FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 12

Dislocations, Plasticity & Recrystallization IV

Recovery, Recrystallization & Grain Growth, Texture & Formability, Dynamic Recrystallization & Superplasticity
TEXTBOOK § 12.10 – § 12.12 · ANNEALING, TEXTURE, FLD & SUPERPLASTICITY · PART 4
“Cold work banks mechanical work inside billions of dislocations, and annealing spends it via migrating boundaries—mastering temperature, strain rate, and orientation tames every grain.”Fundamentals of Materials Science · Ch. 12 · In Tribute to N. P. Goss & M. F. Ashby
Liang Wumse3d.com · Smart Classroom
Top: Strain-free recrystallization nuclei consuming cold-worked matrix · Bottom: Ashby–Verrall 4-grain switching superplasticity
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
OPENING · COLD-WORK STORED ENERGY BRIDGES DISLOCATION THEORY TO MODERN FORMING LINES

Why Does Heating Soften Drawn Wire, While Auto Panels and Transformer Cores Need Opposite Textures?

QUESTION 01 · PURE Cu Trx = 270 °C VS. 500 °C FLASH ANNEAL

Cold drawing dissipates ~90%–99% of work as heat while banking \(1\%\text{–}10\%\) in dislocations—how does annealing relieve stress and rebuild strain-free grains, and why must inline \(\mathrm{Cu}\) wire furnaces run at \(500\,^\circ\mathrm{C}\) for a few seconds?

QUESTION 02 · {111} IF STEEL VS. {110}⟨001⟩ GOSS SILICON STEEL

Why does texture cause wavy “earing” on deep-drawn \(\mathrm{Al}\) cans, whereas car panels seek \(\{111\}\parallel\mathrm{ND}\) and transformer steels target \(\{110\}\langle 001\rangle\)? How do Lankford \(r\), hardening \(n\), and the Forming Limit Diagram (FLD) predict splits?

QUESTION 03 · FLAT DRV IN HOT-ROLLED Al VS. 1000% Ti–6Al–4V

Why is rolling \(\mathrm{Pb}\) at \(25\,^\circ\mathrm{C}\) hot working while \(\mathrm{W}\) at \(1000\,^\circ\mathrm{C}\) is cold working? Why does hot-rolled \(\mathrm{Al}\) show a flat flow plateau while \(\mathrm{Cu}/\gamma\text{-Fe}\) show softening peaks, and how is \(\mathrm{Ti\text{–}6Al\text{–}4V}\) gas-blown into hollow fan blades?

Completing Ch. 12's processing loop: Stored Energy, Recovery, Recrystallization & Grain Growth \(\to\) \(\mathrm{Cu}\)-Wire Flash Annealing \(\to\) Textures, IF/Goss Steels & FLD \(\to\) Dynamic Recrystallization, Superplasticity & Ch. 12 Synthesis.

Textbook § 12.10 – § 12.12 · Processing–Structure–Properties–Performance Loop
§ 12.10 – § 12.12 · FIVE-STOP LECTURE ROADMAP

Guided by Stored Energy \(P\approx\tfrac{1}{2}\rho Gb^2\) & Stacking-Fault Energy Across Cold and Hot Forming

  1. Recovery & Recryst.1%–10% stored energy · subgrains
    \(R^*=2\gamma/P\) & \(T_{\mathrm{rx}}\approx 0.4T_{\mathrm{m}}\)
    § 12.10.1
  2. Grain Growth & WireParabolic \(\bar{d}^2-\bar{d}_0^2=Kt\) · \(\varepsilon_c\)
    \(\mathrm{Cu}\) \(500\,^\circ\mathrm{C}\) flash anneal
    § 12.10.1–12.10.2
  3. Texture, IF & Goss\(\{111\}\) pole figure & ODF
    IF \(\gamma\)-fiber \(r\) & Goss \(\mathrm{Fe\text{–}Si}\)
    § 12.11.1–12.11.2
  4. Forming Limit (FLD)Drawability \(r\) & stretch \(n\)
    Plane-strain trough \(\mathrm{FLC}_0\)
    § 12.11.3
  5. Hot Work & Superplast.\(T_{\mathrm{rx}}\) boundary · DRV/DRX & \(Z\)
    GB sliding \(m\gt 0.3\) & SPF/DB
    § 12.12
Chapter 12 Finale · Preparing for Final Chapter 13: Fracture & Failure of Materials
01
PART ONE

Recovery, Recrystallization & Grain Growth

Cold work dissipates 90%–99% of work as heat while banking 1%–10% in dislocation tangles (\(P\approx\tfrac{1}{2}\rho Gb^2\sim 1\text{ MPa}\)): climb first polygonizes subgrains, then high-angle boundaries sweep the matrix above \((0.35\text{–}0.5)T_{\mathrm{m}}\).
  1. Cold-work stored energy, polygonization recovery, HAGB sweeping & sandbox model05
  2. Normal/abnormal grain growth \(\bar{d}^2-\bar{d}_0^2=Kt\), \(T_{\mathrm{rx}}(\text{K})\) & critical strain \(\varepsilon_c\) hazard06
  3. Cold-draw/anneal cycles, \(\mathrm{Cu}\)-wire \(500\,^\circ\mathrm{C}\) flash annealing (\(100\%\text{ IACS}\)) & AM contrast07
§ 12.10.1 · COLD-WORK STORED ENERGY (1%–10%), POLYGONIZATION RECOVERY & RECRYSTALLIZATION

Recovery Polygonizes Subgrains & Cuts Resistivity; Recrystallization Sweeps via \(P\approx\tfrac{1}{2}\rho Gb^2\), Dropping \(\rho\) \(10^6\times\)

\(\begin{gathered}\text{Recovery }(Q_{\mathrm{rec}}\approx Q_{\mathrm{self}}):\text{climb}\to\textbf{subgrains}\;(\sigma_{\mathrm{res}},\Delta\rho_e\downarrow;\text{ HV }-10\%\text{–}20\%)\\ \text{Recryst.: }P\approx\tfrac{1}{2}\rho Gb^2\sim 1\text{ MPa},\;R^*=\tfrac{2\gamma}{P}\sim 1\;\mu\text{m},\;v=MP,\;X=1-\mathrm{e}^{-kt^n}\end{gathered}\)
  • Stored Energy & Subgrain Nucleation: Only \(1\%\text{–}10\%\) of cold-work energy survives heat dissipation as dislocation stored energy (\(P\sim 1\text{ MPa}\)); during recovery, point-defect annihilation and climb polygonization relieve stress and Matthiessen excess resistivity \(\Delta\rho_e\) while keeping ~85% hardness. Because \(R^*\approx 1\;\mu\text{m}\) far exceeds thermal fluctuations, nuclei form by high-misorientation subgrains growing past \(R^*\).
  • HAGB Sweeping Resets Properties: Strain-free grains bounded by mobile high-angle grain boundaries (HAGBs) sweep the matrix, dropping \(\rho\) from \(10^{16}\) to \(10^{10}\text{ m}^{-2}\) and restoring full ductility.
Textbook § 12.10.1 · Stored Energy P, Polygonization & Critical Radius R* (Fig. 12.28a–c)
§ 12.10.1 · PARABOLIC GRAIN GROWTH d̄² − d̄₀² = Kt, ABNORMAL GROWTH & Trx ≈ (0.35–0.5)Tm

Curvature \(2\gamma/R\) Drives \(10\times\) Slower Coarsening; Heavy Cold Work & High Purity Lower \(T_{\mathrm{rx}}\)

\(\begin{gathered}\frac{\mathrm{d}\bar{d}}{\mathrm{d}t}=M\frac{\alpha\gamma}{\bar{d}}\implies\bar{d}^2-\bar{d}_0^2=Kt\;\;(\bar{d}\propto t^{0.3\text{–}0.5}\text{ w/ drag}),\;\;T_{\mathrm{rx}}\approx(0.35\text{–}0.5)T_{\mathrm{m}}\;(\text{K})\\ 1\text{ h }T_{\mathrm{rx}}:\;\text{pure Fe }450\,^\circ\mathrm{C},\;\text{pure Cu }270\,^\circ\mathrm{C},\;\text{5N Al }100\,^\circ\mathrm{C}\text{ vs. comm. Al }300\,^\circ\mathrm{C}\end{gathered}\)
  • Opposite HAGB Arrows & Secondary Growth (Fig. 12.28c,d): Recrystallizing nuclei bulge away from their center of curvature (pushed by stored \(P\sim 1\text{ MPa}\) against capillarity); once \(P\) is spent, grain boundaries migrate toward their center of curvature under \(2\gamma/R\sim 0.1\text{ MPa}\) via \(\bar{d}^2-\bar{d}_0^2=Kt\) (local unpinning triggers secondary / abnormal grain growth).
  • \(T_{\mathrm{rx}}\) Levers & Critical Strain \(\varepsilon_c\) Hazard: Heavier cold work or finer initial grains lower \(T_{\mathrm{rx}}\), whereas trace solutes drag boundaries to raise \(T_{\mathrm{rx}}\) sharply; straining right near critical strain \(\varepsilon_c\approx 2\%\text{–}10\%\) yields ultra-sparse nuclei that grow into giant coarse grains.
Opposite Boundary Motion (Top) · Trx(K) Levers & Critical Strain εc Hazard (Bottom) (a) Recryst.: Away from Curvature Ctr Strain-free High-ρ matrix Stored P ≈ ½ρGb² (~1 MPa) > 2γ/R (b) Grain Growth: Toward Curvature Ctr Capillarity 2γ/R (~0.1 MPa) · d̄²−d̄₀² = Kt Isochronal Kinetics Trx ≈ (0.35–0.5)Tm (in Kelvin) & Process Warnings: ① Cold work ↑ ⇒ ρ & P ↑ ⇒ Trx ↓, EXCEPT critical strain εc ≈ 2%–10% (abnormal coarse-grain hazard) ② Trace solutes / 2nd-phase particles ↑ ⇒ solute drag & Zener pinning cut M ⇒ Trx jumps +100–300 °C ③ Shorter holding time t ↓ ⇒ requires higher furnace T via t ∝ exp(Q/RT) (inline wire flash anneal) • Secondary / abnormal growth: selective unpinning spawns cm-scale grains (used in Goss Fe–Si)
Textbook § 12.10.1 · Parabolic Grain Growth, Trx(K) & εc Hazard (Fig. 12.28)
§ 12.10.2 & CASE 12.4 · Cu-WIRE CONTINUOUS RESISTANCE FLASH ANNEALING (100% IACS)

Shrinking Dwell Time from \(1\text{ h}\) to \(3.6\text{ s}\) (\(10^{-3}\times\)): Raising \(T\) to \(\sim 500\,^\circ\mathrm{C}\) Buys Back \(10^3\times\) Speed

\(\begin{gathered}\frac{t_2}{t_1}=\exp\!\left[\frac{Q}{R}\!\left(\frac{1}{T_2}-\frac{1}{T_1}\right)\right]\xrightarrow{Q=100\text{ kJ/mol},\;T_1=543\text{ K},\;10^{-3}}T_2\approx 790\text{ K}\;(517\,^\circ\mathrm{C}!)\\ \text{Recrystallized }\rho:10^{16}\to 10^{10}\text{ m}^{-2}\implies\text{conductivity }97\%\to\mathbf{100\%\;\mathrm{IACS}}\end{gathered}\)
  • Answering Q1 (Case 12.4): Pure \(\mathrm{Cu}\) \(T_{\mathrm{rx}}=270\,^\circ\mathrm{C}\;(543\text{ K})\) assumes a \(1\text{ h}\;(3600\text{ s})\) soak; high-speed wire lines use continuous Joule resistance heating for just seconds—with \(Q\approx 100\text{ kJ/mol}\), \(\sim 500\,^\circ\mathrm{C}\) completes recrystallization in seconds (\(450\,^\circ\mathrm{C}\) needs \(\sim 15\text{ s}\)). Requires \(99.95\%\) electrolytic \(\mathrm{Cu}\) to avoid \(\mathrm{Bi/Pb}\) hot shortness and Matthiessen scattering.
  • 3D-Printed Parts Contrast: As-printed AM alloys lack heavy cold work (low stored \(P\)), so annealing targets thermal residual-stress relief and breaking epitaxial \(\langle 001\rangle\) columnar texture rather than classical cold-work recrystallization.
Continuous flash-anneal furnace \(T_2\) (required dwell \(t_2\)): T₂ = 500 °C
Textbook § 12.10.2 & Case 12.4 · Cu-Wire Flash Annealing & 100% IACS
02
PART TWO

Textures, Pole Figures & Sheet Formability

Rolling and annealing align millions of grains—orienting \(\{111\}\parallel\mathrm{ND}\) yields split-free automotive deep-drawing panels, while secondary recrystallization into Goss \(\{110\}\langle 001\rangle\) cuts transformer core losses by \(70\%\).
  1. Wire fiber vs. sheet rolling/recrystallization textures, \(\{111\}\) pole figures & ODFs09
  2. Deep-drawing IF steel \(\gamma\)-fiber \(r\)-value & \(\mathrm{Al}\) can earing vs. Goss electrical steel10
  3. Formability dual metrics (\(r\) vs. \(n\)) & Keeler–Goodwin Forming Limit Diagram (FLD)11
§ 12.11.1 – § 12.11.2 · FIBER VS. SHEET TEXTURES {hkl}⟨uvw⟩, POLE FIGURES & ODFs

Slip Rotates Lattices Toward Principal Axes: Stereographic \(\{111\}\) Pole Clusters Fingerprint Texture

\(\begin{gathered}\text{Wire fiber }\langle uvw\rangle\parallel\text{axis }(\text{fcc }\langle 111\rangle+\langle 100\rangle,\;\text{bcc }\langle 110\rangle)\;\mid\;\text{Sheet }\{hkl\}\langle uvw\rangle\\ \text{Rolling: Cu }\{112\}\langle 111\rangle,\;\text{Brass }\{110\}\langle 112\rangle\;\mid\;\text{Recryst.: Cube }\{100\}\langle 001\rangle,\;\text{Goss }\{110\}\langle 001\rangle\end{gathered}\)
  • Three Origins & Two Tools (Fig. 12.29): Solidification epitaxy, slip-induced lattice rotation, and oriented nucleation/growth all build texture. An XRD or EBSD pole figure stereographically projects one \(\{hkl\}\) family (not area-preserving, so random poles look denser near ND), whereas a 3D Euler-angle \((\varphi_1,\Phi,\varphi_2)\) ODF uniquely resolves full crystal orientations.
Textbook § 12.11.1–12.11.2 · Wire & Sheet Textures, {111} Pole Figures & ODFs (Fig. 12.29)
§ 12.11 EXTENDED READING 1 & 2 · DEEP-DRAWING IF STEEL γ-FIBER VS. GOSS ELECTRICAL STEEL

\(\gamma\)-Fiber \(\{111\}\parallel\mathrm{ND}\) Maximizes Lankford \(r\); \(\mathrm{MnS/AlN}\) Secondary Recrystallization Cuts Core Loss \(70\%\)

\(\begin{gathered}\text{Lankford }r=\frac{\varepsilon_w}{\varepsilon_t}:\;\gamma\text{-fiber }\{111\}\parallel\mathrm{ND}\;(r\approx 2.0\text{–}2.5,\text{ resists thinning})\gg\{100\}\;(r\approx 0.7)\\ \text{Grain-oriented }\mathrm{Fe\text{–}3\%Si}:\;\mathrm{MnS/AlN}\text{ secondary recryst.}\implies\text{Goss }\{110\}\langle 001\rangle\;(\langle 001\rangle\parallel\mathrm{RD})\end{gathered}\)
  • Answering Q2a (IF Steel \(\gamma\)-Fiber & \(\mathrm{Al}\) Can Earing): With \(\{111\}\parallel\mathrm{ND}\), slip resists thickness thinning (\(\varepsilon_t\) tiny \(\Rightarrow r\) high): \(\mathrm{Al}\)-killed steel precipitates \(\mathrm{AlN}\) to block \(\{100\}\) nuclei, while \(\mathrm{Ti/Nb}\)-scavenged IF steel builds strong \(\gamma\)-fiber. In-plane \(\Delta r\neq 0\) causes wavy cup earing (balanced between rolling \(45^\circ\) and Cube \(0^\circ/90^\circ\) ears in \(\mathrm{Al}\) beverage cans).
  • Answering Q2b (Goss Secondary Recrystallization): bcc \(\mathrm{Fe}\) magnetizes easiest along \(\langle 001\rangle\); fine \(\mathrm{MnS/AlN}\) inhibitors Zener-pin primary grains until high-\(T\) coarsening lets rare Goss \(\{110\}\langle 001\rangle\) grains break free into cm-scale crystals, cutting core loss to \(30\%\).
Texture Engineering Twins: IF Deep-Drawing Steel (Left) vs. Goss Transformer Steel (Right) (a) Deep-Drawing Steel: r = εw / εt γ-Fiber {111} ∥ ND (IF Steel r ≈ 2.2) Width flows in easily · resists thinning AlN / Ti(C,N) promote {111} recryst. Planar Δr ≠ 0 ⇒ Wavy Cup “Earing” Al can stock (r ≈ 0.7) balances 0°/90° & 45° ears (b) Grain-Oriented Fe–3%Si: Goss Texture ① Primary Recryst.: MnS/AlN Pinning Normal growth stalled · rare Goss seeds ↓ High-T inhibitor coarsening unpins ↓ ② Secondary Recryst.: {110}⟨001⟩ Easy ⟨001⟩ ∥ Rolling Dir. RD Core loss cut by 70% (to 30% of random) cm-scale grains · abnormal growth crown
Textbook § 12.11 Extended Reading · IF Steel γ-Fiber r-Value & Goss Silicon Steel
§ 12.11.3 · FORMABILITY DUAL METRICS (r VS. n) & KEELER–GOODWIN FORMING LIMIT DIAGRAM (FLD)

Circle Grids Read Out \((\varepsilon_1,\varepsilon_2)\): Plane Strain \(\varepsilon_2=0\) Hits the \(\mathrm{FLC}_0\) Trough & Splits First

\(\begin{gathered}\text{Deep draw }\varepsilon_1\approx -\varepsilon_2\;(\text{flange shear, high }r)\;\mid\;\text{Biaxial stretch }\varepsilon_1=\varepsilon_2\;(\text{delayed neck, high }n)\\ \text{Plane strain }\varepsilon_2=0\implies\text{lowest trough }\mathrm{FLC}_0\;(\text{or }\mathrm{FLD}_0\approx n)\text{ — highest split risk}\end{gathered}\)
  • \(r\) and \(n\) Split Sheet Stamping Duties (Fig. 12.30): Lankford \(r\) governs flange draw-in without sidewall thinning (IF steel \(r\sim 2.5\)), whereas work-hardening exponent \(n\) spreads strain uniformly during biaxial stretching (304 austenitic stainless \(n\sim 0.5\)).
  • Keeler–Goodwin FLD Press-Shop Map: Etched circles deform into ellipses yielding major/minor true strains \((\varepsilon_1,\varepsilon_2)\); punch-nose sidewalls lock width (\(\varepsilon_2=0\)) right at the plane-strain trough \(\mathrm{FLC}_0\), where almost all stampings split first.
Textbook § 12.11.3 · Sheet r/n Metrics, Circle-Grid Strain & Keeler–Goodwin FLD (Fig. 12.30)
03
PART THREE

Dynamic Recrystallization & Superplasticity

Homologous \(T_{\mathrm{rx}}\) divides cold from hot working—stacking-fault energy splits flat DRV plateaus from peaked DRX flow, while sub-\(10\;\mu\text{m}\) grains unlock \(\gt 1000\%\) superplasticity.
  1. Hot vs. cold working (\(\mathrm{Pb}\) vs. \(\mathrm{W}\)), DRV/DRX SFE rule, Zener–Hollomon \(Z\) & TMCP13
  2. Fine-grain superplasticity (\(d\lt 10\;\mu\text{m}\), \(m\gt 0.3\)), Rachinger GBS & \(\mathrm{Ti\text{–}6Al\text{–}4V}\) SPF/DB14
  3. Chapter 12 complete synthesis table & bridge to Chapter 13 Fracture & Failure15
§ 12.12.1 – § 12.12.3 & EXTENDED READING · HOMOLOGOUS Trx BOUNDARY, DRV VS. DRX & PARAMETER Z

High-SFE \(\mathrm{Al}\) Plateaus via DRV, Low-SFE \(\mathrm{Cu}/\gamma\text{-Fe}\) Soften via DRX, and \(Z\) Tunes Peak Count

\(\begin{gathered}T\gt T_{\mathrm{rx}}=\text{hot work }(\text{Pb at }25\,^\circ\mathrm{C}=\text{hot; W at }1000\,^\circ\mathrm{C}=\text{cold})\\ \gamma_{\mathrm{SFE}}\gt 150\;(\mathrm{Al},\alpha\text{-Fe})\to\mathrm{DRV}\mid\gamma_{\mathrm{SFE}}\lesssim 80\;(\mathrm{Cu},\gamma\text{-Fe})\to\mathrm{DRX},\;\;Z=\dot{\varepsilon}\mathrm{e}^{Q/RT}\end{gathered}\)
  • Answering Q3a (Homologous \(T_{\mathrm{rx}}\) & SFE Criterion · Fig. 12.31): Hot working means deforming above \(T_{\mathrm{rx}}\). High-SFE \(\mathrm{Al}\) cross-slips/climbs readily into a flat DRV subgrain plateau; low-SFE \(\mathrm{Cu}/\gamma\text{-Fe}\) pile up dislocations to nucleate DRX softening peaks (high \(Z\) single-peak fine grains vs. low \(Z\) multi-peak cyclic flow).
  • Processing Maps & TMCP Steels: Prasad maps pick high-\(\eta\) DRX domains while avoiding shear bands and wedge cracks; TMCP pancakes \(\gamma\) below its recrystallization stop temperature so accelerated cooling nucleates \(\sim 5\;\mu\text{m}\) ferrite.
Textbook § 12.12.1–12.12.3 · Homologous Hot Work, DRV/DRX, Z & TMCP (Fig. 12.31)
§ 12.12.4 & EXTENDED READING · STRUCTURAL SUPERPLASTICITY, RACHINGER GBS & Ti–6Al–4V SPF/DB

Equiaxed \(d\lt 10\;\mu\text{m}\) Grains Slide & Switch Above \(0.5T_{\mathrm{m}}\): High \(m\approx 0.5\gt 0.3\) Kills Necking

\(\begin{gathered}\text{Three keys: }d\lt 10\;\mu\text{m}\text{ equiaxed},\;\;T\gt 0.5T_{\mathrm{m}},\;\;\dot{\varepsilon}\sim 10^{-4}\text{–}10^{-2}\text{ s}^{-1}\\ \dot{\varepsilon}\propto\frac{D_{\mathrm{gb}}}{d^2}\frac{\sigma^2}{Gk_{\mathrm{B}}T}\implies\sigma=K\dot{\varepsilon}^m,\;\;m=\frac{\partial\ln\sigma}{\partial\ln\dot{\varepsilon}}\approx 0.5\gt 0.3\text{ (blocks necking)}\end{gathered}\)
  • Answering Q3b (Rachinger GBS & Ashby–Verrall Switching · Fig. 12.32): Deformation shifts from intragranular slip to Rachinger grain-boundary sliding (GBS) + diffusive neighbor switching, keeping grains equiaxed past \(1000\%\) elongation. Any incipient neck spikes local \(\dot{\varepsilon}\), raising \(\sigma\propto\dot{\varepsilon}^{0.5}\) (strain-rate hardening) to arrest thinning.
  • Aerospace \(\mathrm{Ti\text{–}6Al\text{–}4V}\) SPF/DB: Slow \(\mathrm{Ar}\)-gas blowing at \(927\,^\circ\mathrm{C}\) combines Superplastic Forming + Diffusion Bonding into hollow wide-chord fan blades and multi-sheet airframe panels in one rivet-free cycle.
Fig. 12.32: Rachinger GBS & Ashby–Verrall Switching (Top) · High m & SPF/DB (Bottom) (1) Initial: A–B Touch C A B D Tensile stress σ → (2) GBS + GB Diffusion Dgb flux heals triple-pt (3) Switched: C–D Touch A C D B 55% stretch · still equiaxed Necking-Resistance Twins & Aerospace Ti–6Al–4V Hollow Fan Blades: • Cold stamping relies on high n (strain hardening σ = Kεⁿ): 20%–60% uniform elongation • Superplasticity relies on high m (rate hardening σ = Kε̇ᵐ, m > 0.3): 500%–2000% elongation • Ti–6Al–4V SPF/DB (927 °C, ε̇ ~ 10⁻³ s⁻¹): Ar-gas blow forming + solid-state diffusion bonding (Note: too fast ε̇ outruns D_gb/d² accommodation, reverting to dislocation slip & early fracture)
Textbook § 12.12.4 · Superplasticity, Rachinger GBS & Ti–6Al–4V SPF/DB (Eq. 12.41, Fig. 12.32)
CHAPTER 12 SYNTHESIS · MECHANICAL STRESS DRIVES SLIP & HARDENING; STORED ENERGY DRIVES ANNEALING

From Single-Dislocation Topological Charge \(\boldsymbol{b}\) to Superplastic Fan Blades — Setting Up Ch. 13

Core ModuleDriving ForceMicro-Carrier & ScaleGoverning Law / CriterionEngineering Payoff
Geometry & ElasticityPeach–Koehler \((\boldsymbol{\sigma}\cdot\boldsymbol{b})\times\boldsymbol{l}\)Edge \(\boldsymbol{l}\perp\boldsymbol{b}\) · Screw \(\boldsymbol{l}\parallel\boldsymbol{b}\) · \(\boldsymbol{b}\)Frank \(E\approx\alpha Gb^2\) · \(\tau b=T/R\)Resolves \(10^4\times\) strength gap
Glide & DissociationEffective \((\tau-\tau_{\mathrm{c}})b\)Glide/climb/cross-slip · \(d\propto 1/\gamma\)\(\tau_{\mathrm{FR}}=Gb/L\) · Lomer–Cottrell lockfcc cryo-tough vs. bcc DBTT
Yield & 4 StrengtheningsSchmid \(\tau_R=\sigma\cos\phi\cos\lambda\)Forest \(\rho^{-1/2}\) · Orowan \(\lambda\) · pile-up \(n\tau\)\(\sigma=M\tau_{\mathrm{c}}\) · \(\varepsilon_u=n\) · \(\sigma_y=\sigma_0+k_y d^{-1/2}\)HSLA, BH/IF steel, T6 Al
Annealing & TextureStored energy \(P\approx\tfrac{1}{2}\rho Gb^2\)Polygonization \(\to\) HAGB \(v=MP\)\(T_{\mathrm{rx}}\approx 0.4T_{\mathrm{m}}\) · \(\bar{d}^2-\bar{d}_0^2=Kt\) · FLDFlash Cu wire, IF & Goss steels
Hot Work & Superplast.High-\(T\) flow + GB diffusionDRV / DRX · Rachinger GBS\(Z=\dot{\varepsilon}\mathrm{e}^{Q/RT}\) · \(\sigma=K\dot{\varepsilon}^m\;(m\gt 0.3)\)TMCP steel, Ti–6Al–4V SPF/DB
Bridge to Final Chapter 13 (Fracture & Failure of Materials): Where plasticity ends, failure begins — ① low-\(T\) bcc screw-core freezing leads directly to Liberty-ship/Titanic DBTT cleavage; ② yield-controlled crack-tip plastic zones govern fracture toughness \(K_{\mathrm{IC}}\); ③ high-\(T\) climb & GB sliding govern power-law creep & grain-boundary cavitation life.
Chapter 12 Synthesis · Dislocation Plasticity Complete, Entering Final Chapter 13
SUMMARY

Stored Energy Resets Cold Work, Texture Tailors IF & Goss Steels, and SFE + Fine Grains Split Hot Forming

Stored P & Subgrains→d̄²−d̄₀²=Kt & Flash Cu→{111} IF & Goss Fe–Si→r · n & FLC₀ Trough→DRX Z & Superplast. m
ANSWERING QUESTIONS 01 & 02

Inline \(\mathrm{Cu}\) wire dwells only seconds, so raising furnace \(T\) to \(500\,^\circ\mathrm{C}\) via \(t\propto\exp(Q/RT)\) completes recrystallization and restores \(100\%\text{ IACS}\); automotive IF steel cultivates \(\{111\}\parallel\mathrm{ND}\) \(\gamma\)-fiber for high Lankford \(r\) while \(\mathrm{MnS/AlN}\) secondary recrystallization builds Goss \(\{110\}\langle 001\rangle\) \(\mathrm{Fe\text{–}Si}\) to cut core loss \(70\%\).

ANSWERING QUESTION 03

Homologous \(T_{\mathrm{rx}}\) makes \(\mathrm{Pb}\) hot-worked at \(25\,^\circ\mathrm{C}\) and \(\mathrm{W}\) cold-worked at \(1000\,^\circ\mathrm{C}\); high-SFE \(\mathrm{Al}\) cross-slips into a flat DRV plateau, whereas sub-\(10\;\mu\text{m}\) \(\mathrm{Ti\text{–}6Al\text{–}4V}\) at \(927\,^\circ\mathrm{C}\) slides along grain boundaries with \(m\approx 0.5\) for rivet-free SPF/DB fan blades.

Next up — Final Chapter 13: Fracture & Failure of Materials — Griffith crack energy balance, fracture toughness \(K_{\mathrm{IC}}\), ductile-to-brittle transition, Paris fatigue crack growth & high-temperature creep.

Dislocations, Plasticity & Recrystallization IV · § 12.10 – § 12.12
CONCEPT QUIZ

Three Quick Questions: Click to Check or Launch a Live Class Poll

1. Pure \(\mathrm{Al}\) melts at \(T_{\mathrm{m}}=933\text{ K}\). Using \(T_{\mathrm{rx}}\approx 0.4T_{\mathrm{m}}\), what is its \(T_{\mathrm{rx}}\)? Why does commercial \(\mathrm{Al}\) anneal much higher while inline \(\mathrm{Cu}\) wire runs at \(500\,^\circ\mathrm{C}\)?

\(0.4\times 933\approx 373\text{ K}\;(\approx 100\,^\circ\mathrm{C})\) in Kelvin. Trace solutes drag boundaries to raise commercial \(\mathrm{Al}\) \(T_{\mathrm{rx}}\), and seconds-scale flash annealing obeys \(t\propto\exp(Q/RT)\).

2. Regarding sheet textures, Lankford \(r\)-value, strain-hardening \(n\), and the Keeler–Goodwin Forming Limit Diagram (FLD), which statement is accurate?

\(\gamma\)-fiber \(\{111\}\parallel\mathrm{ND}\) resists thinning (\(r\approx 2.2\)); \(\mathrm{Fe\text{–}Si}\) uses secondary recrystallization for Goss \(\{110\}\langle 001\rangle\); plane strain \(\varepsilon_2=0\) is the split-prone \(\mathrm{FLC}_0\) trough.

3. Comparing hot-working dynamic recrystallization (DRX) and fine-grain structural superplasticity, which judgment is completely accurate?

High-SFE \(\mathrm{Al}\) undergoes flat DRV; high \(Z\) produces single-peak fine DRX grains; superplasticity relies on Rachinger GBS + diffusion where \(m\approx 0.5\) arrests necking.

Dislocations, Plasticity & Recrystallization IV
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 12 (PART 4) COMPLETE

Thank You

Embedded 2D Model: Annealing: Recovery, Recryst. & Growth (M05·17) — mse3d.com