FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 11

Solid-State Phase Transformations II

Massive Transformation, Pearlite, Bainite, Martensitic Crystallography & Shape-Memory Alloys
TEXTBOOK § 11.6 – § 11.7 · MASSIVE, PEARLITE, BAINITE, MARTENSITE & NITINOL · PART 2
“Phase diagrams mark only the thermodynamic destination; whether atoms diffuse long-range or shear cooperatively decides where a solid microstructure actually stops.”Fundamentals of Materials Science · Ch. 11 · In Tribute to E. C. Bain & T. Y. Hsu (Xu Zuyao)
Liang Wumse3d.com · Smart Classroom
Top: Bain fcc → bct lattice compression & surface relief · Bottom: NiTi thermoelastic martensite detwinning & shape recovery
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
OPENING · FROM LONG-RANGE CARBON DIFFUSION TO SONIC-SPEED COOPERATIVE SHEAR

Why Is Quenched Steel Glass-Brittle, Whereas Bent Nitinol Wire Springs Back on Heating?

QUESTION 01 · EXTREME HARDNESS (HRC 60+) & BRITTLENESS

Slow-cooling \(0.77\%\mathrm{C}\) austenite yields tough pearlitic lamellae, yet water quenching transforms it within \(10^{-7}\text{ s}\)—what interstitial site traps the carbon, and why does growth track cooling rather than isothermal holding?

QUESTION 02 · SUB-0.1 nm SHIFTS & 24 VARIANTS

How does face-centered cubic austenite reconstruct into body-centered tetragonal martensite with atomic shifts under \(0.1\text{ nm}\)? Why can one parent grain spawn up to \(24\) crystallographic variants with visible surface tilt relief?

QUESTION 03 · NITINOL SHAPE MEMORY & 8% SUPERELASTICITY

Heating steel martensite irreversibly tempers it into ferrite plus cementite—how does equiatomic \(\mathrm{NiTi}\) martensite revert reversibly to its parent shape, and even deliver \(8\%\) superelasticity in self-expanding vascular stents?

Along the falling-temperature axis where diffusion freezes out and shear takes over: Massive Transformation & \(T_0\) Locus \(\to\) Pearlite \(\to\) Martensite Thermodynamics & Bain Crystallography \(\to\) Bainite, TRIP Steels & \(\mathrm{NiTi}\).

Textbook § 11.6 – § 11.7 · From Long-Range Diffusion to Cooperative Shear
§ 11.6 – § 11.7 · FIVE-STOP LECTURE ROADMAP

Guided by the \(T_0\) Equal-Free-Energy Locus & \(M_s\) Threshold: Diffusion vs. Shear

  1. Massive & \(T_0\) LocusComposition-invariant jumps
    \(\mathrm{Fe\text{–}C}\) four-zone map
    § 11.6
  2. Pearlite EutectoidLateral \(\mathrm{C}\) partitioning
    Zener law \(\lambda\propto 1/\Delta T\)
    § 11.7.1
  3. Martensite & \(M_s\)T. Y. Hsu interstitial \(\mathrm{C}\)
    Lath/plate & athermal law
    § 11.7.2a
  4. Bain Strain & 24 Var.Embedded \(\sqrt{2}\) bct cell
    IPS habit plane & 24 variants
    § 11.7.2b
  5. Bainite, TRIP & NiTiUpper/lower bainite · TRIP
    Thermoelastic SME & \(8\%\) SE
    § 11.7.3+
Chapter 11 · Part 2 (§ 11.6 – § 11.7) · Foundations for Part 3 TTT/CCT
01
PART ONE

Massive Transform, \(T_0\) Criterion & Pearlite

The \(T_0\) equal-free-energy locus sets the thermodynamic floor for partitionless transformation: above \(T_0\), long-range carbon diffusion grows pearlite lamellae; below \(T_0\), massive short-range jumps and bainite open up.
  1. Massive transformation traits & \(\mathrm{Fe\text{–}C}\) \(A_{\mathrm{e3}} \gt T_0 \gt M_s\) four-zone map05
  2. Table 11.2 four-mechanism comparison: pearlite · massive · bainite · martensite06
  3. Pearlite eutectoid growth & Zener spacing law \(\lambda \approx 2\lambda_{\min} \propto 1/\Delta T\)07
§ 11.6.1 – § 11.6.3 · MASSIVE TRANSFORMATION & THE Fe–C T₀ CRITERION

Below the \(G_\gamma = G_\alpha\) Locus \(T_0\), Atoms Jump Individually Across Incoherent Interfaces

\(\begin{gathered}T_0\text{ locus: }G^\gamma(x_0,T_0)=G^\alpha(x_0,T_0)\;\;(A_{\mathrm{e3}}\gt T_0\gt M_s)\\ v=M_{\mathrm{int}}|\Delta G|\sim 1\text{ cm/s}\;\;(\text{pure Fe window }\sim 10^3\,^\circ\mathrm{C/s})\end{gathered}\)
  • Four Traits of Massive Transformation: ① Composition-invariant (\(x_\alpha=x_\gamma\)); ② Uncoordinated short jumps across incoherent interfaces (patchy grains, zero surface relief!); ③ Interface-mobility controlled (far faster than pearlite); ④ Narrow cooling-rate window (common as massive ferrite in weld HAZ and laser surface hardening).
  • Four \(\mathrm{Fe\text{–}C}\) Temperature Zones (Fig. 11.10): ① \(\gt A_{\mathrm{e3}}\): stable \(\gamma\); ② \(A_{\mathrm{e3}}\text{–}T_0\): partitionless \(\Delta G\gt 0\), so long-range \(\mathrm{C}\) partitioning is mandatory for proeutectoid \(\alpha\); ③ \(T_0\text{–}M_s\): partitionless \(\Delta G\lt 0\) enables massive & bainitic paths; ④ \(\lt M_s\): overcomes shear barrier for martensite.
Select \(0.35\%\mathrm{C}\) steel temp. \(T\): T = 560 °C
Textbook § 11.6.1–11.6.3 · Massive Transform & Fe–C T₀ Four-Zone Map (Fig. 11.10)
§ 11.6.3 TABLE 11.2 · SIX-AXIS COMPARISON OF FOUR SOLID-STATE TRANSFORMATIONS

From \(\mu\text{m/s}\) Diffusion to \(\text{km/s}\) Sonic Shear: Interface Coherency & Surface Relief Compared

FeaturePearlite (Diffusional)Massive (Cross-GB)Bainite (Mixed)Martensite (Displacive)
CompositionChanges (\(\mathrm{C}\) partitions)Unchanged (\(x_\alpha = x_\gamma\))Partial (\(\mathrm{C}\) into \(\gamma\))Unchanged (substitutional)
Atomic MotionLong-range lateral diff.Incoherent short jumps\(\mathrm{Fe}\) shear + short \(\mathrm{C}\) diff.Cooperative lattice shear
Rate Control\(\mathrm{C}\) / alloy diffusionInterface mobility \(M_{\mathrm{int}}\)Mixed (\(\mathrm{C}\)-diffusion limited)Sonic elastic-wave speed
Interface TypeIncoherentIncoherentSemicoherentCoherent / semicoherent
Surface ReliefNoneNone (patchy grains)Yes (invariant-plane tilt)Pronounced tilt relief
Growth Speed\(\sim 1\;\mu\text{m/s}\)\(\sim 10^4\;\mu\text{m/s}\;(1\text{ cm/s})\)\(\sim 1\;\mu\text{m/s}\)\(\approx 10^3\text{ m/s}\;(10^9\;\mu\text{m/s})\)
Growth Speed Spans 9 Orders Pearlite / Bainite (~1 μm/s) Massive Cu–Zn (~10⁴ μm/s) Martensite Sonic Shear (~10⁹ μm/s) Metallographic Shear Test: Pre-polished tilt relief ⇒ shear component
Textbook § 11.6.3 Table 11.2 · Pearlite, Massive, Bainite & Martensite Compared
§ 11.7.1 · PEARLITIC TRANSFORMATION: EUTECTOID COUPLED GROWTH & ZENER SPACING LAW

Interfacial Energy Sets \(\lambda_{\min}\), and Zener Maximum-Velocity Growth Selects \(\lambda \approx 2\lambda_{\min} \propto 1/\Delta T\)

\(\begin{gathered}\gamma_{0.77\%}\xrightarrow{727\,^\circ\mathrm{C}}\alpha_{0.0218\%}+\mathrm{Fe_3C}_{6.69\%},\quad\frac{2\gamma_{\alpha/\mathrm{Fe_3C}}}{\lambda_{\min}}=|\Delta G_v|\approx\frac{\Delta H\,\Delta T}{T_{\mathrm{E}}}\\ \lambda\approx 2\lambda_{\min}=\frac{4\gamma_{\alpha/\mathrm{Fe_3C}}\,T_{\mathrm{E}}}{\Delta H\,\Delta T}\propto\frac{1}{\Delta T},\quad\sigma_y\propto\lambda^{-1/2}\end{gathered}\)
  • Energy Budget & Eutectic Analogy: Each period \(\lambda\) creates two \(\alpha/\mathrm{Fe_3C}\) interfaces—too fine exhausts all driving force on interfacial area, whereas too coarse stalls lateral carbon diffusion, mirroring Ch. 10 Jackson–Hunt coupled eutectic growth.
  • Worked Example: With \(T_{\mathrm{E}}=727\,^\circ\mathrm{C}\), coarse pearlite at \(700\,^\circ\mathrm{C}\) has \(\lambda=0.70\;\mu\text{m}\); lowering to \(600\,^\circ\mathrm{C}\) (\(\Delta T=127\text{ K}\)) refines \(\lambda\) nearly \(5\times\) to \(\mathbf{0.15\;\mu\text{m}}\) (fine / very fine pearlite), sharply boosting Hall–Petch yield strength.
Isothermal pearlite temp. \(T\): T = 650 °C
Textbook § 11.7.1 · Zener Coupled Diffusion & Spacing Law (Eqs. 11.18–11.19)
02
PART TWO

Martensite Thermodynamics & Bain Crystallography

Supersaturated carbon trapped in \(c\)-axis octahedral interstices gives quenched steel its peak hardness, while Bain revealed the hidden two-cell geometric shortcut that turns fcc into bct with sub-\(0.1\text{ nm}\) shifts.
  1. Martensite four traits, T. Y. Hsu's interstitial-\(\mathrm{C}\) refinement & lath vs. plate substructures09
  2. Thermodynamic \(M_s\) threshold, Andrews formula & Koistinen–Marburger athermal kinetics10
  3. Bain strain \(\mathrm{fcc}\to\mathrm{bct}\), invariant-plane strain (IPS) & 24-variant 3D model11
§ 11.7.2 · MARTENSITE TRAITS, T. Y. HSU'S REFINEMENT & LATH VS. PLATE SUBSTRUCTURES

Trapped Carbon Drives \(c/a \gt 1\) Distortion; Low-\(\mathrm{C}\) Forms Dislocation Laths, High-\(\mathrm{C}\) Forms Twinned Plates

\(\begin{gathered}\gamma\text{-Fe (fcc)}\xrightarrow{10^{-7}\text{ s cooperative shear}}\alpha'\text{-Fe (bct)},\quad\frac{c}{a}\approx 1+0.045\,w_{\mathrm{C}}\\ \lt 0.6\%\mathrm{C}:\text{dislocation lath }\alpha'\;\mid\;\gt 1.0\%\mathrm{C}:\text{internally twinned plate }\alpha'\end{gathered}\)
  • Answering Q1 & Four Martensite Traits: Carbon trapped in octahedral interstices stretches \(c/a\) alongside \(10^{15}\text{ m}^{-2}\) dislocations, lifting hardness to HRC 60–65 with severe internal stress. Exhibits diffusionless substitutional lattice (T. Y. Hsu showed interstitial \(\mathrm{C}\) can still partition), sonic speed, athermal kinetics, and surface tilt relief.
  • Carbon Controls Substructure: Low/medium-\(\mathrm{C}\) steels (\(\lt 0.6\%\mathrm{C}\)) form parallel lath packets (tangled dislocations, good toughness); high-\(\mathrm{C}\) steels (\(\gt 1.0\%\mathrm{C}\)) form impinging lenticular plates (fine internal twins, microcrack-prone).
Fig. 11.12c: Low-C Dislocation Lath Packets (Left) vs. High-C Twinned Plates (Right) (a) Lath Martensite (<0.6%C · HRC 55–60) Substructure: 10¹⁵ m⁻² dislocation tangles Thin C-enriched retained γR films (b) Plate Martensite (>1.0%C · HRC ~65) Substructure: nanoscale internal twins High-speed impingement induces microcracks
Textbook § 11.7.2 · T. Y. Hsu, Martensite Traits & Lath/Plate α′ (Eq. 11.20, Fig. 11.12)
§ 11.7.2 · THERMODYNAMIC Ms DEFINITION, ANDREWS FORMULA & ATHERMAL KINETICS

Undercooling Past \(T_0\) Must Bank \(\approx 1250\text{ J/mol}\) for Shear; Each \(0.1\%\mathrm{C}\) Drops \(M_s\) by \(\sim 40\,^\circ\mathrm{C}\)

\(\begin{gathered}\Delta G^{\gamma\to\alpha'}(M_s)=-\Delta G^*_{\mathrm{req}}=-(\Delta G_{\mathrm{strain}}+\Delta G_{\mathrm{int}})\approx -1250\text{ J/mol}\\ M_s(^\circ\mathrm{C})=539-423w_{\mathrm{C}}-30.4w_{\mathrm{Mn}}-\cdots,\;\;f=1-\mathrm{e}^{-0.011(M_s-T)}\end{gathered}\)
  • Why \(M_s\lt T_0\) & Athermal Holding Stops: Cooperative shear must pay an extra elastic-distortion plus interfacial penalty \(\Delta G^*_{\mathrm{req}}\); once cooling stops, driving force \(|\Delta G|\) stops growing, so untransformed \(\gamma\) stalls immediately (athermal kinetics).
  • Carbon Depresses \(M_s\) & Retains Austenite: Dissolved \(\mathrm{C}\) both stabilizes \(\gamma\) and raises tetragonal strain energy; above \(w_{\mathrm{C}}\gt 0.6\%\), \(M_f\) drops below room temperature, inevitably leaving retained austenite \(\gamma_R\).
Carbon content \(w_{\mathrm{C}}\) (quenched to \(25\,^\circ\mathrm{C}\)): 0.80% C
Textbook § 11.7.2 · Ms Barrier, Andrews & Koistinen–Marburger Laws (Eqs. 11.21–11.22)
§ 11.7.2 · MARTENSITIC CRYSTALLOGRAPHY: BAIN STRAIN, INVARIANT HABIT PLANE & 24 VARIANTS

Two Adjacent fcc Cells Embed a \(c/a=\sqrt{2}\) bct Cell: Compress \(c\) by \(17\%\), Expand \(a\) by \(12\%\)

\(\begin{gathered}\text{Bain: }\left(\frac{c}{a}\right)_0=\sqrt{2}\xrightarrow{\varepsilon_c\approx -17\%,\;\varepsilon_a\approx +12\%}\frac{c}{a}\approx 1.05\\ \text{WLR: Bain}+\text{rotation}+\text{LIS (slip/twin)}\implies\text{IPS}\end{gathered}\)
  • Answering Q2 (Minimal Shift & 24 Variants): Every \(\mathrm{Fe}\) atom shifts by under \(0.1\text{ nm}\) while \(\mathrm{C}\) wedges \(c\)-axis octahedral sites; because Bain strain alone leaves no unrotated plane, WLR theory adds rigid-body rotation + lattice-invariant shear (LIS) by slip or twinning across three \(\langle 001\rangle_\gamma\) axes to yield \(24\) crystallographic variants and an invariant habit plane.
  • Carbon-Free Limit: At \(w_{\mathrm{C}}\to 0\) (or after tempering carbide precipitation), \(c\) contracts \(-20\%\) to \(c/a=1.000\) bcc ferrite \(\alpha\).
Textbook § 11.7.2 · Bain Correspondence, Habit Plane & 24 K–S Variants (Fig. 11.11)
03
PART THREE

Bainite, TRIP Steels & Shape-Memory Alloys

Intermediate-temperature para-displacive growth yields tough lower bainite, while harnessing external mechanical work \(W\) or coherent elastic “springs” unlocks crash-resistant TRIP steels and self-expanding Nitinol stents.
  1. Bainitic \(T_0\) incomplete-reaction phenomenon & upper vs. lower bainite toughness13
  2. Extended Reading 1: TRIP steels — mechanical work \(W\) delays necking & doubles \(\sigma\times\varepsilon\)14
  3. Extended Reading 2: Buehler's Nitinol — thermoelastic SME vs. \(8\%\) superelasticity15
§ 11.7.3 · BAINITIC TRANSFORMATION (250–550 °C): T₀ INCOMPLETE REACTION & TOUGHNESS

Carbon Rejection Stalls at the \(T_0\) Curve; Intralath Carbides Make Lower Bainite Ultra-Tough

\(\begin{gathered}T_0\text{ limit: }\alpha_{\mathrm{B}}\text{ rejects C}\to w_{\mathrm{C}}^\gamma\text{ hits }T_0\implies\Delta G\to 0\text{ (stalls)}\\ \text{Upper B }(350\text{–}550\,^\circ\mathrm{C}\text{ interlath)}\;\text{vs.}\;\text{Lower B }(250\text{–}350\,^\circ\mathrm{C}\text{ intralath)}\end{gathered}\)
  • Mixed Para-Displacive Nature: Bainitic ferrite forms via shear (producing surface relief), while growth rate is paced by carbon diffusion; once enriched residual \(\gamma\) reaches the \(T_0\) curve, partitionless driving force vanishes and reaction halts early.
  • Why Springs & Bearings Prefer Lower Bainite: In upper bainite, faster \(\mathrm{C}\) diffusion precipitates coarse \(\mathrm{Fe_3C}\) stringers between laths (easy cleavage); in lower bainite, sluggish \(\mathrm{C}\) precipitates fine \(55^\circ\) carbides inside acicular plates for high strength and toughness.
Upper vs. Lower Bainite Carbides (Top) & Fig. 11.12 Steel Hardness Ladder (Bottom) Upper Bainite (350–550 °C · Feathery) Interlath Fe₃C films → easy cleavage Lower Bainite (250–350 °C · Tough) Fine 55° intralath carbides → high KIC Lower Formation T Freezes C Diffusion → Higher Supersaturation & Dislocations Pearlite (727–550°C) HRC 15–40 · Lamellar Bainite (550–250°C) HRC 40–55 · Fine carb. Martensite (< Ms) HRC 55–65 · Tetragonal
Textbook § 11.7.3 · Bainite T₀ Incomplete Reaction & Upper/Lower Bainite (Fig. 11.12)
§ 11.7 EXTENDED READING 1 · TRIP STEELS (TRANSFORMATION-INDUCED PLASTICITY)

Mechanical Work \(W\) Bridges the \(\Delta G^*\) Gap: Retained Austenite Turns to Martensite Right Where Necking Starts

\(\begin{gathered}\text{Tri-phase: ferrite}+\text{bainite}+\text{C-rich }\gamma_R\;(5\%\text{–}15\%,\;M_s\lt 25\,^\circ\mathrm{C})\\ \bigl|\Delta G^{\gamma\to\alpha'}(T)\bigr|+W_{\mathrm{mech}}\ge\Delta G^*_{\mathrm{req}}\implies\text{strain-induced }\alpha'\text{ (DIM)}\end{gathered}\)
  • Why Retain Metastable \(\gamma_R\) Instead of Quenching Fully? Full martensite cracks during stamping; TRIP steel enriches \(\gamma_R\) with carbon so \(M_s\lt 25\,^\circ\mathrm{C}\), then external stress work \(W\) during stamping or crash impact triggers martensite selectively at incipient necking fronts.
  • Triple Ductility-Toughness Boost: ① Transformation absorbs crash energy; ② fresh hard \(\alpha'\) spikes local work-hardening \(\mathrm{d}\sigma/\mathrm{d}\varepsilon\) to delay necking; ③ \(\sim 4\%\) dilation relaxes crack-tip tension, doubling \(\sigma\times\varepsilon\).
TRIP Mechanism: Mechanical Work W Bridges ΔG* (Left) & Delays Necking (Right) (a) Energy Budget (Ms < T < Md) Threshold ΔG*_req ≈ 1250 J/mol |ΔGchem| Unloaded: stays γR +Work W Neck front: → α′ (b) Tensile Curves & σ × ε Balance Full α′ (early brittle fracture) Conventional HSS TRIP doubles σ × ε Strain ε (delayed necking + 4% dilation) →
Textbook § 11.7 Extended Reading · Automotive TRIP Steels & Strain-Induced Martensite
§ 11.7 EXTENDED READING 2 · BUEHLER'S NITINOL: THERMOELASTIC SME & 8% SUPERELASTICITY

Coherent Interfaces Store Strain as an Elastic “Spring”: Reversible Recovery & \(50\times\) Elastic Strain

\(\begin{gathered}\text{Steel (non-thermoelastic): dislocation plastic relaxation}\implies\text{tempers on heating}\\ \mathrm{NiTi}\text{ (thermoelastic): coherent }\Delta G_{\mathrm{strain}}\text{ spring}\implies\text{reversible }T/\sigma\text{ cycle}\end{gathered}\)
  • Answering Q3 (SME vs. Superelasticity): ① Shape-memory effect (\(T\lt M_f\) bend, heat \(\gt A_f\)): Self-accommodated twins absorb deformation via detwinning without dislocation slip; heating past \(A_f\) forces every variant back to the unique ordered B2 parent crystal.
  • ② Superelasticity (isothermal load–unload at \(T\gt A_f\)): Stress-induced martensite yields a flat plateau and spontaneously reverts upon unloading, recovering up to \(8\%\) strain (\(\sim 50\times\) ordinary metals' \(0.15\%\)) in vascular stents and orthodontic archwires.
Textbook § 11.7 Extended Reading · Buehler's Nitinol, SME & Superelasticity
SUMMARY

\(T_0\) Splits Partitioning from Shear, Bain Finds the Shortest Path, and Coherent Springs Split Steel from NiTi

T₀ Locus & Massive Jumps→Pearlite λ ∝ 1/ΔT→Martensite Ms & C-Wedge→Bain Cell & 24 Variants→Bainite · TRIP · NiTi
ANSWERING QUESTIONS 01 & 02

Quenching traps carbon in \(c\)-axis octahedral sites alongside \(10^{15}\text{ m}^{-2}\) dislocations or twins (HRC 60–65, brittle) and advances athermally as cooling banks \(\Delta G^*_{\mathrm{req}}\); two fcc cells embed a \(c/a=\sqrt{2}\) bct Bain cell that compresses with \(\lt 0.1\text{ nm}\) atomic shifts, coupling with LIS + rotation into \(24\) variants and surface relief.

ANSWERING QUESTION 03

Plastic dislocation relaxation in steel dissipates elastic energy so heating only tempers \(\alpha'\) into \(\alpha+\mathrm{Fe_3C}\); ordered \(\mathrm{NiTi}\) stores transformation strain in coherent interfaces as an elastic “spring,” enabling reversible \(\gt A_f\) shape memory and \(8\%\) superelasticity.

Next lecture turns these mechanisms into engineering heat-treatment maps: Solid-State Phase Transformations III — TTT/CCT diagrams, Jominy hardenability, steel's four classic heat treatments, \(\mathrm{Al}\)-alloy aging windows & the glass transition.

Solid-State Phase Transformations II · § 11.6 – § 11.7
CONCEPT QUIZ

Three Quick Questions: Click to Check or Launch a Live Class Poll

1. Eutectoid steel (\(T_{\mathrm{E}}=727\,^\circ\mathrm{C}\)) forms pearlite with \(\lambda=0.70\;\mu\text{m}\) at \(700\,^\circ\mathrm{C}\); what is \(\lambda\) at \(600\,^\circ\mathrm{C}\)? And if a steel with \(M_s=300\,^\circ\mathrm{C}\) is quenched to \(200\,^\circ\mathrm{C}\) and held isothermally, what is its martensite fraction?

\(\lambda\propto 1/\Delta T\Rightarrow 0.70\times 27/127\approx 0.15\;\mu\text{m}\); \(f=1-\mathrm{e}^{-1.1}\approx 66.7\%\), and athermal martensite does not grow during isothermal holding.

2. Comparing massive transformation, bainite, martensite, and the \(\mathrm{Fe\text{–}C}\) \(T_0\) locus, which statement is completely accurate?

Partitionless \(\gamma\to\alpha\) requires \(T\lt T_0\); massive jumps are uncoordinated (zero relief); each \(0.1\%\mathrm{C}\) drops \(M_s\) by \(\sim 40\,^\circ\mathrm{C}\) and shifts laths to twinned plates.

3. Regarding automotive TRIP steels, Bain crystallography, and biomedical \(\mathrm{NiTi}\) alloys, which judgment is accurate?

Steel \(\alpha'\) relaxes plastically by dislocations and tempers on heating; \(\mathrm{NiTi}\) SE operates above \(A_f\); an invariant habit plane requires Bain strain + LIS + rotation.

Solid-State Phase Transformations II
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 11 (PART 2) COMPLETE

Thank You

Embedded 3D Model: Bain Strain & Martensite Variants (M11·02) — mse3d.com