FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 11 FINALE

Solid-State Phase Transformations III

TTT/CCT Diagrams, Hardenability, Four Principal Heat Treatments, Al-Alloy Aging & Glass Transition
TEXTBOOK § 11.8 – § 11.11 · TTT/CCT, HEAT TREATMENT, AGING & GLASS TRANSITION · PART 3
“Though I had studied the microscopical structure of rocks for many years, I was altogether unprepared for the wonderful complexity of structure which was soon revealed in iron and steel.”Henry Clifton Sorby · J. Iron Steel Inst. (1887)
Liang Wumse3d.com · Smart Classroom
Top: TTT C-curve nose & fast/slow cooling paths · Bottom: crystallization jump Tm vs. kinetic glass freeze-in Tg
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
OPENING · TURNING TIME–TEMPERATURE MAPS INTO STEEL HEAT TREATMENTS, Al AGING & METALLIC GLASSES

How Does One C-Curve Nose Govern Deep-Shaft Hardenability, Temper Toughness & Bulk Metallic Glasses?

QUESTION 01 · WHY DO Cr & Mo HARDEN DEEP CORES WITHOUT RAISING PEAK HRC?

At the water-quenched end, \(0.4\%\;\mathrm{C}\) plain-carbon steel and \(\mathrm{Cr\text{–}Ni\text{–}Mo}\) steel both reach HRC 57–58—why does plain-carbon steel soften past \(8\text{ mm}\), whereas 4340 alloy steel stays martensitic beyond \(50\text{ mm}\)?

QUESTION 02 · WHY MUST STEEL BE QUENCHED & TEMPERED WHILE Al AGES AT ROOM T?

As-quenched steel gears shatter on impact—what four tempering stages trade extreme hardness for toughness, and why does slow cooling past \(500\,^\circ\mathrm{C}\) fall into reversible Type II temper embrittlement?

QUESTION 03 · WHY DO PURE METALS NEED 10¹² K/s FOR GLASS WHILE 5-ELEMENT Zr NEEDS 1 K/s?

Why does the glass transition \(T_{\mathrm{g}}\) shift with cooling rate without latent heat, how do multi-component rules cast \(1.9\text{ GPa}\) bulk metallic glasses, and how does phase-change memory reconcile nanosecond switching with 10-year retention?

Chapter 11 engineering finale: TTT/CCT & Jominy hardenability \(\to\) annealing, normalizing, quenching, four tempering stages & surface hardening \(\to\) Al-alloy T4/T6/T7 aging \(\to\) glass transition & Ch. 11 synthesis.

Textbook § 11.8–11.11 · Process–Structure–Property–Performance
CHAPTER 11 (PART 3) · FIVE-STOP LECTURE ROADMAP

From the C-Curve Nose to Four Principal Heat Treatments, Al-Alloy Aging & Kinetic Vitrification

  1. TTT/CCT & JominyC-curve nose & 5 paths
    End-quench hardenability
    § 11.8
  2. Anneal · Norm. · QuenchFull / spheroidize vs. air
    Martemper & austemper
    § 11.9.1–3
  3. Tempering & Embrittlement\(\varepsilon\)-carbide \(\to\) globular \(\mathrm{Fe_3C}\)
    Type I & II (C-curve TTE)
    § 11.9.4
  4. Surface & Al Aging1045-steel routes & shaft
    Al-alloy T4 / T6 / T7
    § 11.9.5–6
  5. Glass & Ch. 11 Finale\(T_{\mathrm{g}}\), VFT & free volume
    BMG rules & synthesis
    § 11.10–11
Ch. 11 Finale · Next: Ch. 12 Dislocations & Recrystallization
01
PART ONE

TTT / CCT Diagrams & Steel Hardenability

Rotating the bell-shaped nucleation curve by 90° onto a log-time axis yields the master C-curve map of heat treatment: grazing the nose sets the critical cooling rate, while substitutional alloying shifts the nose rightward.
  1. TTT & CCT geometry, five cooling paths & 3D cooling-path workbench05
  2. Hardenability physics (Cr / Mo / Ni nose shift) & Jominy end-quench test06
§ 11.8.1 – § 11.8.2 · ISOTHERMAL (TTT) & CONTINUOUS-COOLING (CCT) DIAGRAMS & 3D WORKBENCH

Bell-Shaped Nucleation Forms the \(550\,^\circ\mathrm{C}\) Nose; Scheil Additivity Shifts CCT Down and Right

\(\begin{gathered}I\propto\mathrm{e}^{-(\Delta G^*+Q)/k_{\mathrm{B}}T}\Rightarrow\text{nose }(550\,^\circ\mathrm{C},1\text{ s}),\;\;\sum\frac{\Delta t_i}{t_s(T_i)}=1\\ v_c\approx\frac{T_\gamma-T_{\mathrm{nose}}}{t_{\mathrm{nose}}}\approx\frac{850-550}{1}=300\,^\circ\mathrm{C/s}\;\;(\text{eutectoid steel})\end{gathered}\)
  • Five Paths Seal the Microstructure: Furnace cool gives coarse pearlite, air cool fine pearlite, oil quench crosses mid-curve into very fine pearlite + martensite, and water quench exceeds \(v_c\) past the nose into martensite + minor \(\gamma_{\mathrm{R}}\); plain eutectoid steel forms zero bainite on continuous cooling—requiring rapid quench + isothermal hold (austempering).
  • Scheil Additivity & Practical Quenching: Consuming incubation fractionally at high \(T\) shifts CCT curves down and right relative to TTT; real quenches need high initial cooling rates at high \(\Delta T\) to clear the curved nose.
Textbook § 11.8.1–11.8.2 · TTT Nose, CCT Shift & Critical Rate (Fig. 11.13)
§ 11.8.2 · HARDENABILITY VS. HARDNESS CAPACITY: SOLUTE DRAG & JOMINY END-QUENCH CURVES

Carbon Sets Peak Hardness, Alloying Sets Depth: \(\mathrm{Cr/Mo/Ni}\) Shift the Nose Right to Harden Thick Cores

\(\begin{gathered}\text{Quenched end }(J=1.6\text{ mm}):\;0.4\%\;\mathrm{C}\text{ steels all hit HRC }57\text{–}58\\ 50\%\text{ martensite depth (HRC 45): }1045\;(7.5\text{ mm})\ll 4140\;(23\text{ mm})\ll 4340\;(\gt 50\text{ mm})\end{gathered}\)
  • Answering Q1 (Why Do Cr, Mo & Ni Boost Hardenability?): Peak martensite hardness depends solely on carbon content; substitutional \(\mathrm{Cr,Mo,Ni}\) diffuse orders of magnitude slower than interstitial \(\mathrm{C}\), requiring long-range partitioning and exerting solute drag (Ch. 9) on boundaries—stretching incubation to shift the C-curve right and slash \(v_c\).
  • Standard Jominy End-Quench Test: One end is water-jet quenched so every axial distance \(J\) experiences a steel-independent cooling rate (\(270\,^\circ\mathrm{C/s}\) at \(1.6\text{ mm}\) down to \(\sim 2\,^\circ\mathrm{C/s}\) at \(45\text{ mm}\)); plotting HRC vs. \(J\) directly quantifies hardenability.
Textbook § 11.8.2 · Hardenability & Jominy Curves (Fig. 11.14)
02
PART TWO

Four Principal Heat Treatments, Surface Hardening & Al Aging

Annealing softens and homogenizes, normalizing refines lamellae in air, quenching locks extreme martensitic hardness, and four tempering stages trade hardness for toughness—joined by case hardening and Al-alloy T4/T6 aging windows.
  1. Four annealing routes (full / spheroidize / stress-relief / recryst.), normalizing & crack-free quenching08
  2. Four tempering stages, high-T tempered martensite (Q&T) & Type I / II temper embrittlement09
  3. Surface hardening, five fates of AISI 1045 steel & shaft process-sequence model10
  4. Al-alloy solution–quench–aging window (T4 natural vs. T6 peak & T7 over-aging)11
§ 11.9.1 – § 11.9.3 · ANNEALING, NORMALIZING & CRACK-FREE QUENCHING

Normalizing Refines 1045-Steel Lamellae to \(0.3\;\mu\text{m}\); Martempering Equalizes \(\Delta T\) Against Quench Cracks

\(\begin{gathered}\text{AISI 1045 full anneal }(\sim 50\,^\circ\mathrm{C/h},\;S_0\approx 0.7\;\mu\text{m},\;\alpha\approx 45\%,\;\text{HB }170)\\ \text{vs. normalizing air cool }(\sim 10\,^\circ\mathrm{C/s},\;S_0\approx 0.3\;\mu\text{m},\;\alpha\approx 30\%,\;\text{HB }200)\end{gathered}\)
  • Four Distinct Annealing Routes: ① Full annealing (hypoeutectoid \(\gt A_{\mathrm{c3}}\) furnace cool to soften); ② Spheroidizing (hypereutectoid \(1.0\%\text{ C}\) tool steel, AISI W1, held near \(A_1\) breaks \(\mathrm{Fe_3C}\) networks into globules, HB ~180 for easy turning); ③ Stress-relief (\(\lt A_1\) recovery); ④ Recrystallization (\(\gt 0.4T_{\mathrm{m}}\) after cold work).
  • Normalizing Trio & Quench-Crack Prevention: Normalizing prevents low-C gummy machining, refines cast/forged coarse grains, and breaks \(\mathrm{Fe_3C_{II}}\) networks; to prevent cracking from thermal + martensitic expansion stresses, replace water quenching with salt-bath martempering (above \(M_s\)) or bainitic austempering.
Figs. 11.15 & 11.16: Four Heat-Treatment Routes (Top) & Three Softening Microstructures (Bottom) A₃ Ms 850 °C Austenitize Quench 600 °C Temper Normalize (Air) Full Anneal (Furnace) Full Anneal (AISI 1045) Thick α network (~45%) Coarse S₀ ≈ 0.7 μm HB ~170 · Cold-extrude Normalizing (AISI 1045) Thin α network (~30%) Fine S₀ ≈ 0.3 μm HB ~200 · Clean cutting Spheroidize (1.0% C W1) Globular Fe₃C in α LSW globules · easy slip HB ~180 · Softest high-C
Textbook § 11.9.1–11.9.3 · Annealing, Normalizing & Quenching (Figs. 11.15–16)
§ 11.9.4 · FOUR TEMPERING STAGES (\(\varepsilon\text{-Fe}_{2.4}\text{C}\to\gamma_{\mathrm{R}}\to\mathrm{Fe_3C}\to\text{GLOBULAR }\mathrm{Fe_3C}\)) & EMBRITTLEMENT

Four Stages Trade Hardness for Q&T Toughness; Fast Cooling Past \(500\,^\circ\mathrm{C}\) Beats \(\mathrm{P/Sb}\) Embrittlement

\(\begin{gathered}\text{I }(100\text{–}250\,^\circ\mathrm{C})\,\varepsilon\text{-carbide}\to\text{II }(200\text{–}300\,^\circ\mathrm{C})\,\gamma_{\mathrm{R}}\text{ decomp.}\to\text{III }(250\text{–}500\,^\circ\mathrm{C})\,\text{med.-}T\text{ tempered }\alpha'\\ \to\text{IV }(500\text{–}650\,^\circ\mathrm{C})\,\mathrm{Fe_3C}\text{ spheroidization}+\alpha\text{ recryst.}=\textbf{high-}T\textbf{ tempered martensite (Q\&T)}\end{gathered}\)
  • Answering Q2 Part 2 (Four Stages): Low-\(T\) tempering follows Ostwald's step rule to precipitate coherent \(\varepsilon\text{-Fe}_{2.4}\text{C}\), relieving stress while keeping HRC ~58–60 (low-\(T\) tempered martensite); medium-\(T\) yields high-elastic-limit medium-\(T\) tempered martensite (springs); high-\(T\) quench & temper (Q&T) yields globular \(\mathrm{Fe_3C}\) + equiaxed \(\alpha\) (high-\(T\) tempered martensite) for peak strength–toughness.
  • Two Embrittlement Minefields: ① Type I (\(250\text{–}400\,^\circ\mathrm{C}\), irreversible): interlath \(\mathrm{Fe_3C}\) films cause an impact trough—never temper here (add \(\mathrm{Si}\) to delay); ② Type II (\(375\text{–}575\,^\circ\mathrm{C}\), reversible): slow cooling lets \(\mathrm{P,Sb,Sn}\) segregate to GBs along a C-curve TTE nose (\(500\text{–}550\,^\circ\mathrm{C}\))—cure by adding \(\mathrm{Mo}\) + rapid cooling after tempering.
Tempering temp. \(T_{\mathrm{temp}}\): 580 °C (Q&T)
Textbook § 11.9.4 · Tempering Stages & Embrittlement (Fig. 11.17)
§ 11.9.5 & CASE STUDY · SURFACE HARDENING & FIVE FATES OF AISI 1045 (0.45% C) STEEL

Induction & Carburizing Build Hard Shells on Tough Cores; Q&T Precedes Finish Machining

\(\begin{gathered}\text{AISI 1045: Anneal }280\text{ MPa}\mid\text{Norm. }340\text{ MPa}\mid\text{Q\&T }\mathbf{620\text{ MPa, }16\%}\\ \text{Shaft: Norm.}\to\text{Rough}\to\textbf{Q\&T}\to\text{Finish}\to\textbf{Induction + Low-}T\textbf{ temper}\end{gathered}\)
  • Dual Surface-Strengthening Routes: High-frequency induction hardening rapidly heats and quenches a \(1\text{–}5\text{ mm}\) skin into low-\(T\) tempered martensite (HRC 52) over a tough Q&T tempered core (HRC 25); carburizing / nitriding diffuse interstitials as \(\delta\sim\sqrt{Dt}\) (nitriding forms ultra-hard nitrides without post-quench distortion).
  • AISI 1045 Shaft Sequence Logic: Q&T (HRC 25) remains machinable, so it goes before finish turning/grinding to lock core toughness and erase roughing stress; induction hardening (HRC 52) goes after finish machining with minimal distortion.
Textbook § 11.9.5 · Surface Hardening & AISI 1045 Process Route
§ 11.9.6 · ALUMINUM-ALLOY HEAT TREATMENT: T4 NATURAL VS. T6 PEAK & T7 AGING WINDOW

Room-\(T\) Vacancies Form Coherent GP Zones (T4); Hitting the \(\theta''\) Ridge Delivers Peak T6 Strength

\(\begin{gathered}\text{Solution + quench }\alpha_{\mathrm{ss}}\xrightarrow{25\,^\circ\mathrm{C}\;\text{T4}}\text{GP zones}\;\mid\;\xrightarrow{160\text{–}190\,^\circ\mathrm{C}\;\text{T6}}\theta''\text{ peak HV}\\ T_{\mathrm{age}}\uparrow\implies D\uparrow\implies\text{earlier }t_{\mathrm{peak}},\text{ but coarser }\bar{r}_{\mathrm{peak}}\text{ & lower peak}\end{gathered}\)
  • Answering Q2 Part 1 (Room-\(T\) Al Hardening vs. Steel Q&T): Aluminum melts at just \(660\,^\circ\mathrm{C}\), so room temperature is already \(\sim 0.32T_{\mathrm{m}}\)—quenched-in excess vacancies drive \(\mathrm{Cu}\) into coherent GP zones within days (T4 natural aging); in steel, room \(T\) only forms Cottrell atmospheres, requiring martensitic quenching + carbide tempering.
  • Under-Aged \(\to\) T6 Peak \(\to\) T7 Over-Aged: Peak strength sits where dislocation shearing meets Orowan looping (\(\theta''\) ridge); aerospace 7075-T73 deliberately slightly over-ages (T7) to defeat stress-corrosion cracking.
Textbook § 11.9.6 · Al-Alloy Solution–Quench–Aging Steps & T4/T6/T7 Tempers
03
PART THREE

Glass Transition, Metallic Glasses & Ch. 11 Synthesis

When cooling outruns even the crystallization C-curve nose, the undercooled liquid surges to a viscosity of \(10^{12}\text{ Pa·s}\) and freezes into an amorphous glass—uniting crystalline and non-crystalline pathways to close Chapter 11.
  1. Kinetic glass transition \(T_{\mathrm{g}}\), Kauzmann paradox, VFT viscosity & free-volume freeze-in13
  2. Turnbull's \(T_{\mathrm{rg}} = T_{\mathrm{g}}/T_{\mathrm{l}}\), Inoue's 3 rules, bulk metallic glasses & PCM memory14
  3. Chapter 11 two-fork master synthesis & bridge into Chapter 12 Dislocations & Plasticity15
§ 11.10.1 – § 11.10.2 · KINETIC GLASS TRANSITION \(T_{\mathrm{g}}\), KAUZMANN PARADOX, VFT VISCOSITY & FREE VOLUME

\(T_{\mathrm{g}}\) Has Zero Latent Heat and Rises with Cooling Rate as \(\eta\to 10^{12}\text{ Pa·s}\) Traps Free Volume

\(\begin{gathered}\eta(T)=\eta_0\exp\!\left(\frac{B}{T-T_0}\right)\;(\text{VFT}),\quad\eta(T_{\mathrm{g}})\approx 10^{12}\text{ Pa·s}\;(\tau\sim 100\text{ s}),\quad\frac{T_{\mathrm{g}}}{T_{\mathrm{m}}}\approx\frac{2}{3}\\ \text{Crystal }(T_{\mathrm{m}}\text{ 1st-order }\Delta V,\Delta H\text{ jump})\;\text{vs.}\;\text{Glass }(T_{\mathrm{g}}\text{ slope kink; fast cool}\Rightarrow\text{higher }T_{\mathrm{g}})\end{gathered}\)
  • Kinetic Freeze-In & Kauzmann's Paradox: Crystallization at \(T_{\mathrm{m}}\) shows discontinuous \(\Delta V\) and latent heat; an undercooled liquid follows Vogel–Fulcher–Tammann (VFT) viscosity surge until relaxation falls behind cooling at \(T_{\mathrm{g}}\) (only a slope kink, zero latent heat), averting the Kauzmann paradox where extrapolated liquid entropy would drop below crystal entropy at \(T_{\mathrm{K}}\).
  • Cohen–Turnbull Free Volume & Relaxation: Faster cooling freezes atomic rearrangement earlier at \(T_{\mathrm{g}2}\gt T_{\mathrm{g}1}\), trapping larger excess free volume \(V_f\) that densifies upon sub-\(T_{\mathrm{g}}\) annealing.
Textbook § 11.10 · Kinetic Tg, VFT & Free Volume (Fig. 11.18)
§ 11.10.2 · TURNBULL'S \(T_{\mathrm{rg}}\), INOUE'S 3 RULES, BULK METALLIC GLASSES & PCM

Deep Eutectics Lift \(T_{\mathrm{rg}} = T_{\mathrm{g}}/T_{\mathrm{l}}\gt 0.6\) for \(1\text{ K/s}\) Vitrification; Zero Dislocations Give \(2\%\) Elastic Limit

\(\begin{gathered}T_{\mathrm{rg}}=\frac{T_{\mathrm{g}}}{T_{\mathrm{l}}}:\;\;\lt 0.5\text{ (pure metal }10^{12}\text{ K/s)}\;\text{vs.}\;\gt 0.6\text{ (Vitreloy 1: }1\text{ K/s!)}\\ \text{Vitreloy 1 }(\mathrm{Zr_{41.2}Ti_{13.8}Cu_{12.5}Ni_{10}Be_{22.5}}):\;\;\sigma_y\approx 1.9\text{ GPa},\;\;\varepsilon_{\mathrm{el}}\approx 2\%\end{gathered}\)
  • Answering Q3 (Inoue's 3 Rules & Confusion Principle): Deep eutectics depress liquidus \(T_{\mathrm{l}}\) to raise \(T_{\mathrm{rg}}=T_{\mathrm{g}}/T_{\mathrm{l}}\), while Inoue's three rules (\(\ge 3\) elements, \(\gt 12\%\) size mismatch, negative \(\Delta H_{\mathrm{mix}}\)) frustrate crystal nucleation (Greer's confusion principle) to push the TTT nose right by 12 orders. Dislocation-free BMGs reach \(2\%\) elastic strain (\(4\times\) steel), while ductile dendrites arrest shear-band localization.
  • Phase-Change Memory Paradox: \(\mathrm{Ge_2Sb_2Te_5}\) melt-quenches into amorphous “0” (RESET) and crystallizes in nanoseconds at the nose for “1” (SET), while high \(T_{\mathrm{g}}\) + fragile VFT steepness lock 10-year room-\(T\) retention.
12-Order Nose Shift: Pure Metal vs. BMG (Left) & Ge₂Sb₂Te₅ PCM Dual Pulses (Right) (a) Inoue Rules Shift Nose Right Tl Tg Pure metal (10¹² K/s) BMG (1 K/s) Log time log t (10⁻⁹ s → 10² s) → (b) PCM Memory (Ge₂Sb₂Te₅) Melt Tm Nose Tx RESET → Amorph. “0” SET → Cryst. “1” Fast nose SET + high-T_g 10-yr lock
Textbook § 11.10.2 · Turnbull Trg, Inoue's 3 Rules, BMGs & PCM
CHAPTER 11 FINALE · TWO PHYSICAL FORKS UNIFY SOLID-STATE TRANSFORMATIONS

Free-Energy Curvature Splits Nucleation vs. Instability; Diffusion vs. Shear Sets Speed—Next Up: Dislocations

Transformation FamilyFree-Energy Curvature / BarrierAtomic Migration ChannelSignature Kinetics & ScaleEngineering Applications
Precipitation & Pearlite\(G''\gt 0\) · barrier incl. \(\Delta G_{\mathrm{strain}}\)Long-range diffusion (\(\sqrt{Dt}\) / lateral)Avrami \(1-\mathrm{e}^{-kt^n}\) · LSW \(\bar{r}^3\propto t\) · \(\lambda\propto\Delta T^{-1}\)Al T4/T6, anneal / norm. / Q&T steels
Spinodal Decomp.\(G''\lt 0\) · zero-barrier instabilityUphill diffusion (\(\tilde{D}\lt 0\))Cahn \(\beta(k)\) · nano-wavelength \(\lambda_m=2\pi/k_m\)Modulated alloys, Alnico magnets
Massive & BainiteUndercooled below \(T_0\) (\(G^\alpha=G^\gamma\))Incoherent jump / shear + \(\mathrm{C}\) diffusion\(v=M_{\mathrm{int}}|\Delta G|\) · \(T_0\) incomplete reactionWeld HAZ massive \(\alpha\), bearing lower bainite
Martensite & FerroicOvercomes \(\Delta G^*_{\mathrm{req}}\) or Landau double wellDiffusionless cooperative shear / shift24 Bain/K–S variants · \(E_c\) switching · Curie–WeissQuenched/TRIP steel, \(\mathrm{NiTi}\), PZT, \(\mathrm{Nd_2Fe_{14}B}\)
Glass TransitionKinetic freeze-in (no \(\Delta H\), no \(\Delta V\))VFT viscosity surge freezes free volume\(\eta(T_{\mathrm{g}})\approx 10^{12}\text{ Pa·s}\) · \(T_{\mathrm{rg}}=T_{\mathrm{g}}/T_{\mathrm{l}}\)Vitreloy BMGs, amorphous cores, PCM
Bridge to Ch. 12 Dislocations, Plastic Deformation & Recrystallization: Chapters 1–11 tracked thermally driven diffusion, interface migration, and phase shear; Chapter 12 brings applied mechanical stress onto center stage to reveal the fourth atomic channel—dislocation glide—governing yield strength, work hardening, strengthening mechanisms, and annealing recrystallization.
Textbook § 11.11 · Ch. 11 Master Synthesis & Bridge to Ch. 12
SUMMARY

Steer the Four Heat Treatments by C-Curves, Balance Q&T Toughness, and Freeze Free Volume into Glass

TTT/CCT & Jominy→Anneal · Norm. · Quench→4 Temper Stages & TTE→1045 Steel & Al T4/T6→Glass Transition & BMGs
ANSWERING QUESTIONS 01 & 02

Peak HRC at the quenched end is set by carbon, whereas substitutional \(\mathrm{Cr,Mo,Ni}\) partition slowly and exert solute drag to shift the TTT nose right, hardening thick shaft cores; quenched steel requires four tempering stages to precipitate carbides for toughness (fast-cooled past \(500\,^\circ\mathrm{C}\) with \(\mathrm{Mo}\) to prevent \(\mathrm{P/Sb}\) Type II embrittlement), whereas Al at room \(T\approx 0.32T_{\mathrm{m}}\) clusters coherent GP zones via quenched-in vacancies (T4).

ANSWERING QUESTION 03

\(T_{\mathrm{g}}\) marks kinetic freeze-in at \(\eta\approx 10^{12}\text{ Pa·s}\) (zero latent heat, higher upon fast cooling) that averts Kauzmann's paradox; multi-component deep eutectics obeying Inoue's rules lift \(T_{\mathrm{rg}}=T_{\mathrm{g}}/T_{\mathrm{l}}\gt 0.6\) to cast dislocation-free \(1.9\text{ GPa}\) bulk metallic glasses at \(1\text{ K/s}\).

Chapter 11 complete. Up next — Chapter 12 · Dislocations, Plastic Deformation & Recrystallization: theoretical shear strength gap, Burgers vector, Frank–Read sources, and the four strengthening mechanisms.

Solid-State Phase Transformations III · End of Chapter 11
CONCEPT QUIZ

Three Quick Questions: Click to Check or Launch a Live Class Poll

1. A steel austenitized at \(850\,^\circ\mathrm{C}\) has its TTT nose at \((1\text{ s},\,550\,^\circ\mathrm{C})\): what is \(v_c\)? And why does AISI 4340 (\(\mathrm{Ni\text{–}Cr\text{–}Mo}\)) steel harden far deeper than AISI 1045 (\(0.45\%\text{ C}\)) steel?

\(v_c\approx(850-550)/1=300\,^\circ\mathrm{C/s}\); carbon sets max HRC, while substitutional \(\mathrm{Cr,Ni,Mo}\) slow decomposition and shift the nose right.

2. Which process plan for an AISI 1045 (\(0.45\%\text{ C}\)) drive shaft and temper-embrittlement control is completely sound?

High-\(T\) tempered martensite (Q&T, HRC 25) machines cleanly before induction hardening (HRC 52); \(\mathrm{Mo}\) + fast cooling past \(500\,^\circ\mathrm{C}\) prevents \(\mathrm{P/Sb}\) Type II embrittlement.

3. Which statement accurately characterizes the glass transition \(T_{\mathrm{g}}\) and bulk metallic glasses (BMGs)?

\(T_{\mathrm{g}}\) rises with cooling rate with no latent heat or \(\Delta V\); dislocation-free BMGs reach ~\(2\%\) elastic limit and deform via localized shear bands.

Solid-State Phase Transformations III
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 11 COMPLETE

Thank You

Embedded Models: TTT / CCT Cooling Path Workbench · Four Fates of the Same Steel · Aging Precipitation Window — mse3d.com