FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 12

Dislocations, Plasticity & Recrystallization III

Schmid's Law, Work Hardening, Cottrell Atmospheres & Strengthening Mechanisms
TEXTBOOK § 12.6 – § 12.9 · DISLOCATIONS, PLASTICITY & RECRYSTALLIZATION · PART 3
“Packing obstacles closer raises the dislocation bowing threshold Gb/L across every alloy—yet grain refinement alone strengthens a metal while simultaneously preserving its toughness.”Fundamentals of Materials Science · Ch. 12 · In Tribute to Schmid, Cottrell, Hall & Petch
Liang Wumse3d.com · Smart Classroom
Top: Schmid resolved shear stress & single-crystal slip activation · Bottom: Eshelby pile-up stress concentration & Hall–Petch grain refinement
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
PROLOGUE · FROM SINGLE DISLOCATIONS TO COLLECTIVE GLIDE, ENTANGLEMENT & STRENGTHENING LAWS

How Does Orientation Set Yielding, Why Do Lüders Bands Form, and Why Does Only Grain Refinement Toughen?

QUESTION 1 · CRYSTAL ORIENTATION VS. POLYCRYSTAL M̄ = 3.06

Pulling pure Cu single crystals from the same melt along different axes yields wildly different tensile yield stresses \(\sigma_y\)—what microscopic threshold stays invariant? And why must each polycrystal grain activate at least \(5\) independent slip systems, making it ~1.5× stronger than a soft single crystal?

QUESTION 2 · WORK HARDENING, YIELD DROP & 45° CREASES

More dislocations should ease slip, so why does cold bending harden iron wire? Why do automotive mild-steel sheets receive a \(1\%\text{–}3\%\) skin-pass temper roll before stamping, yet suffer \(45^\circ\) surface creases again after three months in storage?

QUESTION 3 · FOUR STRENGTHENING ROUTES & NANOSCALE LIMIT

Solid-solution, precipitation, and forest hardening all scale with \(\Delta\tau\propto Gb/L\): why does Hall–Petch obey \(d^{-1/2}\) instead of \(d^{-1}\), uniquely raising both strength and toughness—yet reverse and soften below \(10\text{–}20\text{ nm}\)?

This lecture connects the four pillars of macroscopic plasticity: true stress–strain & Schmid/Taylor laws \(\to\) work hardening & Considère necking \(\to\) Cottrell atmospheres & Lüders bands \(\to\) four strengthening mechanisms & inverse Hall–Petch.

Ch. 12 § 12.6–§ 12.9 · Yielding, Necking & Strengthening Models
§ 12.6 – § 12.9 · FIVE STOPS LINKING SLIP GEOMETRY, NECKING INSTABILITY & POLYCRYSTAL STRENGTHENING

One Critical Resolved Shear Stress Thread Across Schmid Projection, Forest Hardening & Pile-Ups

  1. True Stress & Taylor\(\sigma=s(1+e),\;\varepsilon=\ln(1+e)\)
    Von Mises 5 systems & \(\bar{M}\)
    § 12.6.1 & 12.6.3
  2. Schmid's Law\(m=\cos\phi\cos\lambda\le 0.5\)
    Soft/hard axes & overshoot
    § 12.6.2 & 12.6.4
  3. Hardening & NeckingStages I–III (\(\theta_{\mathrm{II}}\approx G/300\))
    Considère \(\varepsilon_u=n\) & \(\sqrt{\rho}\)
    § 12.7
  4. Cottrell & AgingUYP/LYP & 45° Lüders band
    Skin-pass, IF, BH & PLC
    § 12.8
  5. Four StrengthenersShearing \(r^{1/2}\) vs. Orowan \(Gb/\lambda\)
    Hall–Petch \(d^{-1/2}\) & HSLA
    § 12.9
Ch. 12 Part 3 of 4 · Covering § 12.6–§ 12.9 & HSLA Steel Case
01
PART I

True Stress–Strain, Schmid's Law & Taylor Factor

Separate true strain hardening from post-necking engineering load drop, project axial tension twice onto a slip system via Schmid's factor \(m\), and see how neighbor compatibility enforces 5 independent slip systems with Taylor factor \(\bar{M}=3.06\).
  1. Engineering vs. true stress–strain, \(0.2\%\) offset yield, lattice rotation & Taylor factor \(\bar{M}=3.06\)05
  2. Schmid's law \(\tau_{\mathrm{R}}=\sigma\cos\phi\cos\lambda\ge\tau_{\mathrm{c}}\), \(m_{\max}=0.5\) & slip activation model06
§ 12.6.1 & § 12.6.3 · TRUE VS. ENGINEERING STRESS–STRAIN, VON MISES 5 SYSTEMS & TAYLOR FACTOR M̄

True Stress Keeps Rising Past Necking; Neighbor Compatibility Enforces 5 Systems and \(\sigma_y = 3.06\tau_{\mathrm{c}}\)

\(\begin{gathered}\varepsilon=\ln(1+e),\quad\sigma=s(1+e)\;\;[\sigma_t=\sigma_e(1+\varepsilon_e),\;\text{const. vol. }Al=A_0l_0]\\ \text{von Mises }\varepsilon_{11}+\varepsilon_{22}+\varepsilon_{33}=0\implies\ge 5\text{ indep. systems};\;\;\sigma_y=\bar{M}\tau_{\mathrm{c}}\;(\bar{M}_{\mathrm{fcc}}=3.06)\end{gathered}\)
  • True vs. Engineering Curves & \(\sigma_{0.2}\): Metals lacking a sharp yield drop define proof strength via the \(0.2\%\) plastic-offset line \(\sigma_{0.2}\); after necking (\(A\ll A_0\)), engineering stress \(s=\sigma_e=F/A_0\) falls while true stress \(\sigma=\sigma_t=F/A\) keeps hardening.
  • Answering Q1 Part 2 (Why \(\bar{M}=3.06\gt 2\)?): A soft single crystal (\(m=0.5\)) yields at \(\sigma_y=2\tau_{\mathrm{c}}\) on a single system, whereas each polycrystal grain constrained by surrounding neighbors must simultaneously activate \(\ge 5\) independent slip systems (many unfavorably oriented), lifting random fcc yield to \(\bar{M}\tau_{\mathrm{c}}=3.06\tau_{\mathrm{c}}\) (fcc has \(5\) independent systems for ductility; hcp basal slip has only \(2\), causing polycrystal brittleness).
True σ vs. Engineering s Curve (Left) & Polycrystal Taylor Compatibility M̄ = 3.06 (Right) (a) 0.2% Offset & Post-Necking Split True σ = Kεⁿ (hardens) Eng. s = F/A₀ (neck drop) UTS (εu = n) 0.2% offset σ₀.₂ (b) Soft Single Crystal vs. Polycrystal Free Single Crystal (Soft m = 0.5) Only 1 primary slip system needed σy = τc / 0.5 = 2.00 τc Random Polycrystal (Constrained) 6 strains − const. vol. ⇒ 5 indep. strains Must co-activate ≥ 5 indep. systems fcc: σy = M̄ τc = 3.06 τc
Textbook § 12.6.1 & 12.6.3 · True Stress–Strain & Taylor Factor M̄
§ 12.6.2 & § 12.6.4 · SCHMID'S LAW τR = σ cos φ cos λ ≥ τc, LATTICE ROTATION & SLIP ACTIVATION MODEL

Force Projection \(\cos\lambda\) Times Area Projection \(\cos\phi\) Peaks at \(m_{\max}=0.5\) for \(45^\circ\)

\(\begin{gathered}\tau_{\mathrm{R}}=\frac{F\cos\lambda}{A_0/\cos\phi}=\sigma\cos\phi\cos\lambda=m\sigma\ge\tau_{\mathrm{c}},\;\;\sigma_y=\frac{\tau_{\mathrm{c}}}{m}\;\;(\phi+\lambda\ge 90^\circ)\\ \phi=\lambda=45^\circ\Rightarrow m_{\max}=0.5\text{ (soft)}\;\mid\;\phi=90^\circ\text{ or }\lambda=90^\circ\Rightarrow m=0\text{ (locked)}\end{gathered}\)
  • Answering Q1 Part 1: Regardless of how \(\sigma_y\) varies with orientation, single-crystal Cu yields at an invariant critical resolved shear stress \(\tau_{\mathrm{c}}=m\sigma_y\approx 0.5\text{ MPa}\). At \(\phi=\lambda=45^\circ\) (\(m=0.5\)), \(\sigma_y=1.0\text{ MPa}\); at \(\phi=60^\circ,\;\lambda=38^\circ\) (\(m\approx 0.394\)), \(\sigma_y\) climbs to \(1.27\text{ MPa}\).
  • Multislip, Lattice Rotation & Overshoot: Pulling along \([001]\) co-activates \(8\) systems (\(m=0.408\)) for immediate hardening; single-slip axes rotate toward \(\langle 110\rangle\) under grip constraint and overshoot the \([001]\text{–}[111]\) symmetry boundary via latent hardening before conjugate slip.
Textbook § 12.6.2 & 12.6.4 · Schmid's Law, Lattice Rotation & Overshoot
02
PART II

Work Hardening, Considère Necking & Cottrell Atmospheres

Multiplying dislocations entangle into a dense forest that raises flow stress as \(\sqrt{\rho}\); necking strikes the instant hardening rate drops to true stress, while interstitial C/N clouds stage upper/lower yielding and \(45^\circ\) Lüders bands.
  1. Three-stage single-crystal hardening, Hollomon law \(\sigma=K\varepsilon^n\) & Considère necking model08
  2. Taylor forest relation \(\Delta\tau=\alpha Gb\sqrt{\rho}\), intersection jogs, Lomer–Cottrell locks & TWIP09
  3. Cottrell C/N atmospheres, upper/lower yield points & \(45^\circ\) Lüders band propagation10
  4. Strain aging, \(1\%\text{–}3\%\) skin-pass rolling, IF & bake-hardening steels, and PLC blue brittleness11
§ 12.6.1 & § 12.7.1 · SINGLE-CRYSTAL STAGES I–III, HOLLOMON LAW σ = Kεⁿ & CONSIDÈRE CRITERION

Load Peaks When \(\mathrm{d}\sigma/\mathrm{d}\varepsilon = \sigma\): Uniform True Necking Strain Equals \(\varepsilon_u = n\)

\(\begin{gathered}\text{Stage I easy glide}\to\text{Stage II linear }\theta_{\mathrm{II}}\approx G/300\to\text{Stage III cross-slip recovery}\\ \mathrm{d}F=0\iff\frac{\mathrm{d}\sigma}{\mathrm{d}\varepsilon}=\sigma\xrightarrow{\sigma=K\varepsilon^n}\varepsilon_u=n,\;\;e_u=\mathrm{e}^n-1\end{gathered}\)
  • Microscopic Origin of Stages I–III (Fig. 12.22): Stage I single slip glides long distances; Stage II multislip forest intersections & L–C locks set a universal slope \(\theta_{\mathrm{II}}\approx G/300\); Stage III screw cross-slip bypasses obstacles (low-SFE austenitic stainless steel suppresses cross-slip, prolonging Stage II with \(n\approx 0.48\)).
  • Considère Subtangent Rule: Necking starts precisely when subtangent \(\sigma/\theta=1\); higher \(n\) lets incipiently thinned spots self-harden and extends uniform elongation.
Textbook § 12.6.1 & 12.7.1 · Stages I–III & Considère Necking (Eq. 12.29)
§ 12.7.1 – § 12.7.2 · TAYLOR FOREST LAW Δτ = αGb√ρ, JOGS, L–C LOCKS & TWIP STEELS

A \(10^6\times\) Surge in Density Shrinks Forest Spacing to \(\rho^{-1/2}\), Boosting Strength \(10^3\times\)

\(\begin{gathered}l_{\mathrm{forest}}\approx\rho^{-1/2}\xrightarrow{\Delta\tau\approx Gb/l}\tau=\tau_0+\alpha Gb\sqrt{\rho}\;\;(\alpha\approx 0.3)\\ \text{Worked check: }\rho:10^{10}\to 10^{15}\text{ m}^{-2}\;(G=48\text{ GPa},\;b=0.25\text{ nm})\implies\Delta\tau\approx 114\text{ MPa}\end{gathered}\)
  • Answering Q2 Part 1 (Four Hardening Mechanisms): ① Parallel pile-up repulsion; ② Forest intersections leaving energy-costly jogs and kinks while spacing \(l\approx\rho^{-1/2}\) forces \(\alpha Gb\sqrt{\rho}\) bow-out; ③ Sessile Lomer–Cottrell locks sealing \(\{111\}\) slip corridors; ④ Stage III self-organized high-density dislocation cell walls.
  • TWIP (Twinning-Induced Plasticity) Steels: Low-SFE high-Mn austenitic steels continuously nucleate nanoscale deformation twins that slice grains finer during pulling (dynamic Hall–Petch), sustaining high \(\theta\) to delay necking past \(50\%\) elongation.
Textbook § 12.7.1–12.7.2 · Taylor Forest Law, Jogs & TWIP Steels (Eq. 12.30)
§ 12.8.1 – § 12.8.2 · COTTRELL ATMOSPHERES, UPPER/LOWER YIELD POINTS & 45° LÜDERS BANDS

Interstitial C/N Clouds Pin Edge Cores, Causing Yield Drop and \(45^\circ\) Lüders Sweep

\(\begin{gathered}E_{\mathrm{int}}=-\sigma_{\mathrm{h}}\Delta V_{\mathrm{s}}:\;\Delta V_{\mathrm{s}}\gt 0\;(\mathrm{C,N,Mo})\to\text{tension}\;\mid\;\Delta V_{\mathrm{s}}\lt 0\;(\mathrm{Si})\to\text{compression}\\ \text{Upper yield }\sigma_{\mathrm{uy}}\text{ (unpinning)}\longrightarrow\text{Lower yield }\sigma_{\mathrm{ly}}\text{ (45° Lüders plateau)}\end{gathered}\)
  • Answering Q2 Part 2 (Figs. 12.23 & 12.24): Trace interstitial C and N segregate into the dilated tensile zone beneath positive edge cores to relieve misfit strain and lock dislocations; axial stress must peak at the upper yield point \(\sigma_{\mathrm{uy}}\) to unpin (or multiply fresh mobile dislocations), then drops to the lower yield point \(\sigma_{\mathrm{ly}}\).
  • \(45^\circ\) Lüders Bands & Stretcher Strains: Localized yield bands at \(\sim 45^\circ\) (maximum shear) sweep from specimen shoulders across the entire gauge before uniform hardening starts, marring stamped auto body panels with unsightly stretcher-strain creases.
Textbook § 12.8.1–12.8.2 · Cottrell Atmospheres & Lüders Bands
§ 12.8.3 · STRAIN AGING, SKIN-PASS TEMPER ROLLING, IF/BH STEELS & PLC BLUE BRITTLENESS

\(1\%\text{–}3\%\) Skin-Pass Rolling Erases Creases; \(170\,^\circ\mathrm{C}\) Paint Baking Re-Pins for Dent Resistance

\(\begin{gathered}\text{Skin-pass }(1\%\text{–}3\%)\implies\text{fresh mobile }\perp\text{ erase plateau}\;\;(\text{3-mo storage}\Rightarrow\text{strain aging})\\ v_{\mathrm{diff}}\approx v_{\mathrm{disl}}\;(200\text{–}300\,^\circ\mathrm{C}\text{ steel})\implies\text{repeated re-pinning}=\text{PLC serrations & blue brittleness}\end{gathered}\)
  • Two Remedies Against Creases: ① Light skin-pass temper rolling (\(1\%\text{–}3\%\)) injects unpinned mobile dislocations for smooth yielding, but sheets must be stamped promptly before room-temperature strain aging restores C/N clouds; ② Scavenging all free C/N with trace \(\mathrm{Ti/Nb}\) yields non-aging interstitial-free (IF) steel with strong \(\{111\}\) deep-drawing texture.
  • Bake Hardening (BH) vs. PLC Blue Brittleness: BH auto sheets retain trace solute C to stamp softly without creases, then re-pin during \(170\,^\circ\mathrm{C}\times 20\text{ min}\) paint baking (\(+\,40\text{–}60\text{ MPa}\) dent resistance). Conversely, working steel at \(200\text{–}300\,^\circ\mathrm{C}\) lets diffusing C/N repeatedly catch moving dislocations (Portevin–Le Chatelier dynamic strain aging), causing serrated flow and blue brittleness.
Engineering Cottrell Clouds: Skin-Pass · Bake Hardening · IF Steel · PLC Blue Brittleness (a) 1%–3% Skin-Pass Temper Rolling Fresh mobile ⊥ → smooth yield (b) Bake-Hardening (BH) Steel (170 °C) +40–60 MPa BH Soft in stamping · hard after bake (c) Interstitial-Free (IF) Steel (Ti/Nb) TiC/NbC Zero free C/N atoms Non-aging + strong {111} Deep-drawn auto panels (r ≈ 2.2) (d) Dynamic Aging: PLC & Blue Brittle Pin → unpin → re-catch (serrations) Avoid forging at 200–300 °C blue zone
Textbook § 12.8.3 · Strain Aging, IF/BH Steels & Blue Brittleness
03
PART III

Four Strengthening Mechanisms & Inverse Hall–Petch

Solutes, precipitates, and forest dislocations all tighten bowing spacing \(L\); grain boundaries alone amplify stress via \(n\)-dislocation pile-ups to yield the \(d^{-1/2}\) law—powering tough HSLA steels until grain-boundary sliding takes over below \(10\text{–}20\text{ nm}\).
  1. Solid-solution mismatch \(\Delta\tau\propto c^{1/2}\) & coherent shearing vs. Orowan looping 3D model13
  2. Eshelby pile-up \(\tau_{\mathrm{tip}}=n\tau^*\), Hall–Petch \(d^{-1/2}\) & nanocrystalline inverse Hall–Petch model14
  3. Case 12.3: HSLA microalloyed steel four-term strengthening budget & low DBTT15
  4. Four strengthening mechanisms compared: why grain refinement alone raises toughness16
§ 12.9 & § 12.9.1 · BOWING FAMILY Gb/L, SOLID-SOLUTION Δτ ∝ c¹/² & SHEARING VS. OROWAN 3D MODEL

Fine Particles Shear (\(\propto r^{1/2}\)), Coarse Particles Loop (\(\tau\approx Gb/\lambda\propto 1/r\)): Peak Aging Hits at \(r^*\)

\(\begin{gathered}\sigma_y=\sigma_0+\Delta\sigma_{\mathrm{ss}}(\propto c^{1/2})+\Delta\sigma_{\mathrm{ppt}}+\Delta\sigma_{\mathrm{gb}}+\Delta\sigma_{\mathrm{wh}}\\ \text{Shearing }\Delta\tau\propto r^{1/2}\;\;\text{vs.}\;\;\tau_{\mathrm{Orowan}}\approx\frac{Gb}{\lambda}\propto\frac{1}{r}\;\;(\lambda=50\text{ nm}\Rightarrow 400\text{ MPa})\end{gathered}\)
  • Unified \(Gb/L\) Bowing Family & Solid Solution: F–R sources \(Gb/L\), Orowan \(Gb/\lambda\), forest \(\alpha Gb\sqrt{\rho}\), and solid-solution pinning (\(L\propto c^{-1/2}\Rightarrow\Delta\tau\propto c^{1/2}\) from atomic size + modulus mismatch, e.g., \(\mathrm{Cu\text{–}Be}\) bronze) all obey line-tension bowing.
  • Peak-Aging Lower Envelope (Fig. 12.25): Dislocations select whichever path costs less—shearing coherent particles (creating steps + APBs, \(\propto r^{1/2}\)) vs. Orowan looping (\(\propto 1/r\) at fixed volume fraction), peaking at \(r^*\approx 5\text{ nm}\) before coarsening over-ages.
Textbook § 12.9 & 12.9.1 · Solid Solution, Shearing & Orowan Bypass
§ 12.9.2 – § 12.9.3 · DISLOCATION PILE-UP τtip = nτ*, HALL–PETCH d⁻¹/² & INVERSE HALL–PETCH

Pile-Up Count \(n\propto\tau^* d\) Concentrates Tip Stress \(n\tau^*\propto(\tau^*)^2 d\implies d^{-1/2}\); Below \(15\text{ nm}\), GBs Slide

\(\begin{gathered}n\approx\frac{\tau^* d}{Gb}\;(\tau^*=\tau-\tau_0),\;\;\tau_{\mathrm{tip}}=n\tau^*=\frac{(\tau^*)^2 d}{Gb}=\tau_{\mathrm{crit}}\implies\sigma_y=\sigma_0+k_y d^{-1/2}\\ \text{Larson–Miller check: }50\;\mu\text{m }(199\text{ MPa})\to\mathbf{1\;\mu\text{m }(800\text{ MPa})};\;\;d\lt d_c\;(10\text{–}20\text{ nm})\Rightarrow\text{GB sliding}\end{gathered}\)
  • Answering Q3 Part 1 (Origin of \(d^{-1/2}\)): Effective shear stress \(\tau^*=\tau-\tau_0\) enters twice—setting both pile-up count \(n\propto\tau^* d\) and force per dislocation—so finer grains hold fewer dislocations, weaken tip leverage, and demand higher applied stress \(\sigma_y=\sigma_0+k_y d^{-1/2}\).
  • Inverse Hall–Petch Below \(10\text{–}20\text{ nm}\): When \(d\lt d_c\approx 10\text{–}20\text{ nm}\), grains cannot fit pile-ups while boundary volume \(f_{\mathrm{gb}}\approx 3\delta/d\) hits \(\sim 30\%\), switching deformation to grain-boundary sliding softening (plus thermal coarsening & zero work hardening).
Textbook § 12.9.2–12.9.3 · Pile-Up & Direct/Inverse Hall–Petch Laws
§ 12.9.2 CASE 12.3 · HSLA MICROALLOYED STEEL: HOW 0.02%–0.1% Nb/V/Ti LIFTS 235 MPa STEEL TO ~600 MPa

Zener Pinning Refines Ferrite to \(5\;\mu\text{m}\) While Nanoscale \(\mathrm{NbC/VN}\) Adds Orowan Strength

\(\begin{gathered}\sigma_y^{\mathrm{HSLA}}=\sigma_{\mathrm{base}}(235)+\Delta\sigma_{\mathrm{gb}}(+160)+\Delta\sigma_{\mathrm{Orowan}}(+150)+\Delta\sigma_{\mathrm{ss}}(+40)\\ \approx 585\text{ MPa}\;\;(\text{measured }420\text{–}690\text{ MPa, while lowering DBTT to }-45\,^\circ\mathrm{C!})\end{gathered}\)
  • Linear Superposition via Trace Microalloying: ① Hot-rolling austenite: undissolved \(\mathrm{NbC/TiN}\) Zener-pins boundaries during TMCP, refining transformed ferrite from \(20\;\mu\text{m}\) to \(5\;\mu\text{m}\) (\(d^{-1/2}\) doubles, adding \(+160\text{ MPa}\)); ② Cooling transformation: \(2\text{–}10\text{ nm}\) \(\mathrm{NbC/VN}\) precipitates add \(+100\text{–}200\text{ MPa}\) Orowan strength; ③ \(\mathrm{Mn/Si}\) solid solution adds \(+30\text{–}50\text{ MPa}\).
  • Low-Carbon Structural Workhorse: Eliminates costly wt%-level \(\mathrm{Ni/Cr}\) additions and quench-and-temper heat treatments across bridges, Arctic pipelines, and crash-resistant chassis.
Textbook § 12.9.2 Case 12.3 · HSLA Steel Superposition & Toughness
§ 12.9 SYNTHESIS · SOLID-SOLUTION, PRECIPITATION, WORK HARDENING & GRAIN REFINEMENT SYNTHESIS

Three Routes Trade Ductility for Strength; Grain Refinement Alone Raises Both Strength and Toughness

MechanismCore Dislocation ObstacleScaling LawDuctility & Toughness (DBTT)Engineering Examples
Solid-SolutionSolute size & modulus misfit fields pin/drag dislocations\(\Delta\tau\propto c^{1/2}\) (dilute \(\propto c\))Strength \(\uparrow\) · elongation & toughness dip slightly\(\mathrm{Cu\text{–}Zn}\) brass, \(\mathrm{Cu\text{–}Be}\), 5xxx Al–Mg
Second-PhaseCoherent shearing (steps + APB) vs. Orowan loopingShear \(\propto r^{1/2}\); Orowan \(\tau\approx Gb/\lambda\)Strength \(\uparrow\uparrow\) · peak-aged toughness drops markedly7xxx/2xxx T6 Al, maraging steel, 17-4PH
Work HardeningForest intersections (jogs), L–C locks & dense cell walls\(\tau=\tau_0+\alpha Gb\sqrt{\rho}\)Strength \(\uparrow\uparrow\) · remaining uniform \(e_u\) falls sharplyCold-drawn piano wire, Cu wire, rolled SS
Grain RefinementGBs block slip, shrinking pile-up count \(n\) & tip stress\(\sigma_y=\sigma_0+k_y d^{-1/2}\) (\(d\gt d_c\))Strength \(\uparrow\uparrow\) AND toughness rises (lowers DBTT)HSLA pipeline steel, TMCP ultrafine steel
Answering Q3 Part 2 (“Strengthening” \(\ne\) “Toughening”): As-quenched martensite and heavy cold work raise \(\sigma_y\) sharply yet exhaust mobile dislocation capacity and shrink crack-tip plastic zones, inviting brittle fracture; grain refinement alone raises \(\sigma_y\) via shorter pile-ups while blunting grain-boundary stress concentration and deflecting cleavage cracks across high-angle boundaries to lower DBTT.
Textbook § 12.9 · Four Strengthening Mechanisms & Toughness
SUMMARY

Schmid Projection Sets Yielding, Considère Predicts Necking, and \(Gb/L\) + \(d^{-1/2}\) Govern Strengthening

Schmid m & M̄ = 3.06→Stages I–III & εu = n→Cottrell & 45° Lüders→Shear r¹/² vs. Gb/λ→Hall–Petch d⁻¹/²
ANSWERING QUESTIONS 1 & 2

Single crystals yield at invariant \(\tau_{\mathrm{R}}=m\sigma_y=\tau_{\mathrm{c}}\) (\(m_{\max}=0.5\) at \(45^\circ\)), while neighbor-constrained polycrystals require \(5\) independent slip systems (\(\sigma_y=3.06\tau_{\mathrm{c}}\)); forest intersections harden metals via \(\alpha Gb\sqrt{\rho}\), and C/N Cottrell unpinning stages mild-steel yield drops and \(45^\circ\) Lüders bands.

ANSWERING QUESTION 3

Solutes, Orowan particles, and forest dislocations all set \(Gb/L\) bowing thresholds, whereas grain boundaries leverage \(n\)-dislocation pile-ups (\(\tau_{\mathrm{tip}}=n\tau^*\propto(\tau^*)^2 d\)) to yield \(d^{-1/2}\)—uniquely raising both strength and toughness until \(d\lt 10\text{–}20\text{ nm}\) triggers grain-boundary sliding.

Next Lecture (Chapter 12 Finale) — Dislocations, Plasticity & Recrystallization IV: recovery, recrystallization & grain growth, crystallographic texture & forming limit diagrams (FLD), dynamic recrystallization (DRX), and superplasticity.

Dislocations, Plasticity & Recrystallization III
CONCEPT QUIZ

Three Quick Questions: Click an Option to Check or Launch a Live Class Poll

1. Single-crystal Cu is pulled at \(\phi=45^\circ,\;\lambda=45^\circ\) with \(\tau_{\mathrm{c}}=0.5\text{ MPa}\): what is \(\sigma_y\), and how many independent slip systems does von Mises polycrystal compatibility require?

Since \(m=\cos 45^\circ\cos 45^\circ=0.5\), \(\sigma_y=\tau_{\mathrm{c}}/m=1.0\text{ MPa}\); plastic volume constancy leaves \(6-1=5\) independent strain components.

2. Given \(G=80\text{ GPa},\;b=0.25\text{ nm}\) and non-shearable spacing \(\lambda=50\text{ nm}\), what is \(\tau_{\mathrm{Orowan}}\)? And for \(\sigma=K\varepsilon^{0.35}\), at what true strain \(\varepsilon_u\) does necking start?

\(\tau_{\mathrm{Orowan}}\approx Gb/\lambda\) gives \(80\text{ GPa}\times 0.25\text{ nm}/50\text{ nm}=400\text{ MPa}\); Considère's criterion yields \(\varepsilon_u=n=0.35\).

3. For steel with \(\sigma_0=100\text{ MPa}\) and \(k_y=0.7\text{ MPa·m}^{1/2}\), what is \(\sigma_y\) at \(d=1\;\mu\text{m}\), and how are mild-steel stamping Lüders creases prevented?

At \(d=1\;\mu\text{m}\), \(d^{-1/2}=1000\text{ m}^{-1/2}\), so \(\sigma_y=100+0.7\times 1000=800\text{ MPa}\); prolonged storage triggers strain aging and restores creases.

Dislocations, Plasticity & Recrystallization III
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 12 (PART 3)

Thank You

6 Embedded Models: Schmid Factor · Work Hardening & Necking · Dislocation Intersection & Reactions · Cottrell Atmosphere & Yield Point · Cutting & Orowan Bypass · Hall–Petch Pile-up — mse3d.com